An environmentally friendly polyacrylate lithium battery adhesive tape
By using the polyacrylate lithium battery adhesive tape prepared with specific proportional materials and treatment steps, the problem of insufficient resistance of existing lithium battery adhesive tape in high temperature and electrolyte is solved, and better stickiness and resistance are achieved High temperature performance improves the safety of lithium battery manufacturing.
Patent Information
- Application Number
- CN202310197313.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-03-03
AI Technical Summary
The lack of resistance of existing lithium battery adhesive tapes in high temperatures and electrolytes has limited the promotion and application of lithium battery manufacturing.
Butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, dodecane Aluminum sulfate, EG emulsifier and ethyl acetate are prepared by specific mixing and treatment methods, including stirring, constant temperature of water bath, drying and cooling. Steps to improve its viscosity and high temperature resistance.
The prepared lithium battery adhesive tape has good adhesive holding performance and high temperature resistance, which improves the safety of the adhesive tape and significantly improves its adhesive performance at high temperature.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyacrylate materials, and in particular to an environmentally friendly polyacrylate lithium battery adhesive tape. Background Art
[0002] With the continuous development of the country in new energy and energy conservation and emission reduction, products such as pure electric vehicles and smart phones are developing rapidly, and the corresponding market demand for high-performance lithium batteries is growing rapidly. In the production process of lithium batteries, processes such as electrode winding, tab protection, core termination and shell protection to prevent electrolyte leakage require the use of high-temperature and electrolyte-resistant adhesive tapes.
[0003] Adhesive tape is made of paper, cloth, or film as the base material, and glue is evenly coated on the above base material to make paper adhesive tape, cloth adhesive tape, or film adhesive tape. According to the adhesive properties, it can be divided into solvent-based adhesive tape, emulsion adhesive tape, hot-melt adhesive tape, calendered adhesive tape, and reactive adhesive tape.
[0004] At present, the types of lithium battery pressure-sensitive adhesives commonly used in the market are mainly solvent-based rubber, silicone and acrylate. Solvent-based pressure-sensitive adhesives have the disadvantages of solvent volatilization, pollution and poor safety, while emulsion-based acrylic acid pressure-sensitive adhesives have the advantages of environmental protection, safety, non-toxicity and low cost. However, in the application of lithium battery tapes, its poor electrolyte and temperature resistance and the strict requirements of lithium battery manufacturing process on water content limit its promotion and application. Therefore, the development and preparation of high temperature resistant and electrolyte resistant hydrophobic functional adhesive tapes has a good practical guiding significance for the manufacture of lithium batteries. Summary of the invention
[0005] To this end, the present invention provides an environmentally friendly polyacrylate lithium battery adhesive tape, and the preparation method thereof comprises the following steps:
[0006] (1) mixing butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium lauryl alcohol ether sulfate, EG emulsifier and ethyl acetate to obtain a mixture A;
[0007] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, mixing 1 / 5 to 1 / 6 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, and keeping the mixture in a water bath at a constant temperature of 80±3° C. and stirring for 30 to 40 minutes. After the stirring is completed, the remaining mixture A is added to the mixture under stirring. After the addition is completed, the mixture is kept at 80±3° C. and stirred for 4 to 5 hours. After the stirring is completed, the temperature is lowered to 70±5° C. and kept at a temperature of more than 1 hour, and then air-cooled to room temperature to obtain mixture B;
[0008] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120-130° C. for 2-3 min, and then transferred to an oven at 60±2° C. for more than 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0009] Furthermore, the preparation method of the amino-modified emulsion is:
[0010] Step 1, preparing an aqueous solution of sodium hydroxide, mixing N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate to form a mixture, and heating the mixture to 80±3° C. in a water bath for 5 to 6 hours, and then air-cooling to 60±3° C. to obtain a mixture C;
[0011] Step 2: prepare a composite aqueous solution of epichlorohydrin and acetone, add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a heat preservation state of 60±3°C, stir for more than 10 hours under a heat preservation state of 60±3°C after the addition is completed, add tri(3-aminopropyl)amine after the stirring is completed, stir for more than 10 hours under a heat preservation state of 60±3°C after the addition is completed, and air cool to room temperature to obtain the amino-modified emulsion.
[0012] Furthermore, the mixed weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are respectively: 120 to 150 parts of butyl acrylate, 20 to 24 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 80 to 100 parts of amino-modified emulsion, 10 to 16 parts of dipropylene glycol diacrylate, 20 to 25 parts of methyl methacrylate, 10 to 12 parts of ammonium dodecyl alcohol ether sulfate, 10 to 15 parts of EG emulsifier and 200 to 250 parts of ethyl acetate.
[0013] Furthermore, in the aqueous solution of ammonium persulfate and ammonium bicarbonate, the concentration of ammonium persulfate is 20-30 g / L, the concentration of ammonium bicarbonate is 12-16 g / L, and the solvent is water; the mass ratio of 1 / 5-1 / 6 of the mixture A and the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A: aqueous solution of ammonium persulfate and ammonium bicarbonate = 10:2-3.
[0014] Furthermore, in the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 10-15 g / L, and the solvent is water; the mixing mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:4-6:0.3-0.4:2-5.
[0015] Furthermore, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin:acetone:water=4-6:50:50-60; the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone=1:1-2.
[0016] Furthermore, the mass ratio of the added mass of the tris(3-aminopropyl)amine to the mixture C is mixture C:tris(3-aminopropyl)amine=1:0.12-0.18.
[0017] The beneficial effect of the present invention is that the lithium battery adhesive tape prepared by the method of the present invention has good adhesive holding performance and high temperature resistance, thereby improving the safety of the adhesive tape in use. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the embodiments.
[0019] Example 1
[0020] An environmentally friendly polyacrylate lithium battery adhesive tape, the preparation method of which comprises the following steps:
[0021] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 120 parts of butyl acrylate, 20 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 80 parts of amino-modified emulsion, 10 parts of dipropylene glycol diacrylate, 20 parts of methyl methacrylate, 10 parts of ammonium dodecyl alcohol ether sulfate, 10 parts of EG emulsifier and 200 parts of ethyl acetate;
[0022] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 20 g / L and the concentration of ammonium bicarbonate is 12 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:2; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0023] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0024] The preparation method of the amino-modified emulsion is as follows:
[0025] Step 1, preparing an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 10 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:4:0.3:2; the mixture is heated to 80±3° C. in a water bath, kept warm for 5 hours, and then air-cooled to 60±3° C. to obtain a mixture C;
[0026] Step 2, prepare a composite aqueous solution of epichlorohydrin and acetone, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin: acetone: water = 4:50:50; add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a 60±3°C insulation state, the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone = 1:1; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, add tris(3-aminopropyl)amine after the stirring is completed, and the mass ratio of the added mass of tris(3-aminopropyl)amine to the mixture C is mixture C: tris(3-aminopropyl)amine = 1:0.12; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, and air cool to room temperature to obtain the amino-modified emulsion.
[0027] Example 2
[0028] An environmentally friendly polyacrylate lithium battery adhesive tape, the preparation method of which comprises the following steps:
[0029] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 130 parts of butyl acrylate, 22 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 90 parts of amino-modified emulsion, 12 parts of dipropylene glycol diacrylate, 22 parts of methyl methacrylate, 11 parts of ammonium dodecyl alcohol ether sulfate, 13 parts of EG emulsifier and 200 parts of ethyl acetate;
[0030] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 20 g / L and the concentration of ammonium bicarbonate is 14 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:2; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0031] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0032] The preparation method of the amino-modified emulsion is as follows:
[0033] Step 1, preparing an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 12 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:5:0.3:3; the mixture is heated to 80±3° C. in a water bath, kept warm for 5 hours, and then air-cooled to 60±3° C. to obtain a mixture C;
[0034] Step 2, prepare a composite aqueous solution of epichlorohydrin and acetone, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin: acetone: water = 5:50:50; add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a 60±3°C insulation state, the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone = 1:1; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, add tris(3-aminopropyl)amine after the stirring is completed, and the mass ratio of the added mass of tris(3-aminopropyl)amine to the mixture C is mixture C: tris(3-aminopropyl)amine = 1:0.14; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, and air cool to room temperature to obtain the amino-modified emulsion.
[0035] Example 3
[0036] An environmentally friendly polyacrylate lithium battery adhesive tape, the preparation method of which comprises the following steps:
[0037] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 140 parts of butyl acrylate, 22 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 90 parts of amino-modified emulsion, 14 parts of dipropylene glycol diacrylate, 24 parts of methyl methacrylate, 11 parts of ammonium dodecyl alcohol ether sulfate, 13 parts of EG emulsifier and 200 parts of ethyl acetate;
[0038] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 30 g / L and the concentration of ammonium bicarbonate is 14 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:3; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0039] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0040] The preparation method of the amino-modified emulsion is as follows:
[0041] Step 1, preparing an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 13 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:5:0.4:4; the mixture is heated to 80±3° C. in a water bath, kept warm for 5 hours, and then air-cooled to 60±3° C. to obtain a mixture C;
[0042] Step 2, prepare a composite aqueous solution of epichlorohydrin and acetone, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin: acetone: water = 5:50:50; add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a 60±3°C insulation state, the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone = 1:1; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, add tris(3-aminopropyl)amine after the stirring is completed, and the mass ratio of the added mass of tris(3-aminopropyl)amine to the mixture C is mixture C: tris(3-aminopropyl)amine = 1:0.16; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, and air cool to room temperature to obtain the amino-modified emulsion.
[0043] Example 4
[0044] An environmentally friendly polyacrylate lithium battery adhesive tape, the preparation method of which comprises the following steps:
[0045] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 150 parts of butyl acrylate, 24 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 100 parts of amino-modified emulsion, 16 parts of dipropylene glycol diacrylate, 25 parts of methyl methacrylate, 12 parts of ammonium dodecyl alcohol ether sulfate, 15 parts of EG emulsifier and 200 parts of ethyl acetate;
[0046] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 30 g / L and the concentration of ammonium bicarbonate is 16 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate / ammonium bicarbonate aqueous solution = 10:3; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0047] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0048] The preparation method of the amino-modified emulsion is as follows:
[0049] Step 1, preparing an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 15 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:6:0.4:5; the mixture is heated to 80±3° C. in a water bath, kept warm for 5 hours, and then air-cooled to 60±3° C. to obtain a mixture C;
[0050] Step 2, prepare a composite aqueous solution of epichlorohydrin and acetone, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin: acetone: water = 6:50:50; add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a 60±3°C insulation state, the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone = 1:1; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, add tris(3-aminopropyl)amine after the stirring is completed, and the mass ratio of the added mass of tris(3-aminopropyl)amine to the mixture C is mixture C: tris(3-aminopropyl)amine = 1:0.18; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, and air cool to room temperature to obtain the amino-modified emulsion.
[0051] Comparative Example 1
[0052] A comparative adhesive tape, the preparation method of which comprises the following steps:
[0053] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 130 parts of butyl acrylate, 22 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 12 parts of dipropylene glycol diacrylate, 22 parts of methyl methacrylate, 11 parts of ammonium dodecyl alcohol ether sulfate, 13 parts of EG emulsifier and 200 parts of ethyl acetate;
[0054] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 20 g / L and the concentration of ammonium bicarbonate is 14 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:2; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0055] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0056] Comparative Example 2
[0057] A comparative adhesive tape, the preparation method of which comprises the following steps:
[0058] (1) butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are mixed and stirred uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 130 parts of butyl acrylate, 22 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 90 parts of emulsion, 12 parts of dipropylene glycol diacrylate, 22 parts of methyl methacrylate, 11 parts of ammonium dodecyl alcohol ether sulfate, 13 parts of EG emulsifier and 200 parts of ethyl acetate;
[0059] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 20 g / L and the concentration of ammonium bicarbonate is 14 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:2; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0060] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0061] The preparation method of the emulsion in this comparative example is as follows: prepare an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 12 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:5:0.3:3; the mixture is heated to 80±3°C in a water bath, kept warm for 5 hours, and then air-cooled to 60±3°C and kept warm to obtain a mixture C as the emulsion in this comparative example.
[0062] Comparative Example 3
[0063] A comparative adhesive tape, the preparation method of which comprises the following steps:
[0064] (1) mixing butyl acrylate, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium lauryl alcohol ether sulfate, EG emulsifier and ethyl acetate and stirring them uniformly to obtain a mixture A; the weight proportions of the butyl acrylate, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium lauryl alcohol ether sulfate, EG emulsifier and ethyl acetate are as follows: 130 parts of butyl acrylate, 90 parts of amino-modified emulsion, 12 parts of dipropylene glycol diacrylate, 22 parts of methyl methacrylate, 11 parts of ammonium lauryl alcohol ether sulfate, 13 parts of EG emulsifier and 200 parts of ethyl acetate;
[0065] (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the concentration of ammonium persulfate is 20 g / L and the concentration of ammonium bicarbonate is 14 g / L, and the solvent is water; mixing 1 / 5 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, wherein the mass ratio of 1 / 5 of the mass of mixture A to the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A:ammonium persulfate and ammonium bicarbonate aqueous solution = 10:2; placing the mixture in a water bath at a constant temperature of 80±3° C., maintaining the temperature at 60 r / min, and stirring for 30 min; adding the remaining mixture A to the mixture under stirring after the stirring is completed; continuing to maintain the temperature at 80±3° C., maintaining the temperature at 60 r / min, and stirring for 4 h; cooling the mixture to 70±5° C., maintaining the temperature for 1 h, and then air cooling the mixture to room temperature to obtain mixture B;
[0066] (3) The mixture B is coated on a PET film by a coating machine, and then dried at 120° C. for 3 min, and then transferred to an oven at 60±2° C. for 20 h, and then air-cooled to room temperature to obtain the lithium battery adhesive tape.
[0067] The preparation method of the amino-modified emulsion is as follows:
[0068] Step 1, preparing an aqueous solution of sodium hydroxide, wherein the concentration of sodium hydroxide in the aqueous solution of sodium hydroxide is 12 g / L, and the solvent is water; N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate are uniformly mixed to form a mixture, wherein the mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:5:0.3:3; the mixture is heated to 80±3° C. in a water bath, kept warm for 5 hours, and then air-cooled to 60±3° C. to obtain a mixture C;
[0069] Step 2, prepare a composite aqueous solution of epichlorohydrin and acetone, the volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin: acetone: water = 5:50:50; add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a 60±3°C insulation state, the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone = 1:1; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, add tris(3-aminopropyl)amine after the stirring is completed, and the mass ratio of the added mass of tris(3-aminopropyl)amine to the mixture C is mixture C: tris(3-aminopropyl)amine = 1:0.14; after the addition is completed, stir at 60r / min for 10h under a 60±3°C insulation state, and air cool to room temperature to obtain the amino-modified emulsion.
[0070] Example 5
[0071] The adhesive tapes prepared by the methods described in the above embodiments and comparative examples were measured for their long-lasting adhesion and high temperature resistance. The dry adhesive thickness of the samples prepared in the embodiments and comparative examples was 0.6 mm. The long-lasting adhesion was tested in accordance with the requirements of the national standard GB / T4851-2014. The samples were cut into square samples of 25 mm × 100 mm and then bonded to the surface of a stainless steel plate that met the standard requirements. After bonding, they were rolled 3 times with a 2 kg roller, left to stand for 30 seconds, and then the falling time of each tape was tested with a 1 kg weight according to the standard requirements, as the long-lasting adhesion of the group of samples. The test method for high temperature resistance is: cut the sample into several square samples of 25mm×100mm, and then stick them on the surface of the stainless steel plate that meets the requirements of GB / T4851-2014 standard. After sticking, use a 2 kg roller to roll 3 times, let it stand for 30s, and then put several stainless steel plates with samples into an oven at 100-250℃ (set a group every 10℃) and bake for 1 hour. After baking, take out the stainless steel plate and slowly tear off the sample to see if there is any residual glue on the surface of the steel plate. The highest baking temperature without residual glue is the high temperature resistance of this group of samples. The results are shown in Table 1. As can be seen from Table 1, the lithium battery adhesive tape prepared by the method of the present invention has good persistent adhesion and high temperature resistance, which improves the safety of the adhesive tape. The experiment found that by adding the amino-modified emulsion of the present invention to the adhesive tape raw material, the persistent adhesion and high temperature resistance of the adhesive tape can be significantly improved. This may be because the amino-modified emulsion can promote the crosslinking and dispersion of molecules in the adhesive tape, which is manifested macroscopically as the improvement of the continuous adhesion and high temperature resistance of the adhesive tape.
[0072] Table 1
[0073] Experimental Group Stickiness(h) High temperature resistance(℃) Example 1 93 210 Example 2 95 220 Example 3 94 220 Example 4 91 200 Comparative Example 1 39 130 Comparative Example 2 57 160 Comparative Example 3 80 180
[0074] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. An environmentally friendly polyacrylate lithium battery adhesive tape, characterized in that: The preparation method comprises the following steps: (1) mixing butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium lauryl alcohol ether sulfate, EG emulsifier and ethyl acetate to obtain a mixture A; (2) preparing an aqueous solution of ammonium persulfate and ammonium bicarbonate, mixing 1 / 5 to 1 / 6 of the mass of mixture A with the aqueous solution of ammonium persulfate and ammonium bicarbonate, and placing the mixture in a water bath at a constant temperature of 80±3° C. and stirring for 30 to 40 minutes. After the stirring is completed, the remaining mixture A is added to the mixture under stirring. After the addition is completed, the mixture is kept at 80±3° C. and stirred for 4 to 5 hours. After the stirring is completed, the mixture is cooled to 70±5° C. and kept at this temperature for more than 1 hour, and then air-cooled to room temperature to obtain mixture B; (3) coating the mixture B on a PET film using a coating machine, drying the film at 120-130° C. for 2-3 min, placing the film in an oven at 60±2° C. for more than 20 h, and then air cooling the film to room temperature to obtain the lithium battery adhesive tape; The preparation method of the amino-modified emulsion is: Step 1, preparing an aqueous solution of sodium hydroxide, mixing N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate to form a mixture, and heating the mixture to 80±3° C. in a water bath for 5 to 6 hours, and then air-cooling to 60±3° C. to obtain a mixture C; Step 2: prepare a composite aqueous solution of epichlorohydrin and acetone, add the composite aqueous solution of epichlorohydrin and acetone to the mixture C under a heat preservation state of 60±3°C, stir for more than 10 hours under a heat preservation state of 60±3°C after the addition is completed, add tri(3-aminopropyl)amine after the stirring is completed, stir for more than 10 hours under a heat preservation state of 60±3°C after the addition is completed, and air cool to room temperature to obtain the amino-modified emulsion.
2. The environmentally friendly polyacrylate lithium battery adhesive tape according to claim 1, characterized in that: The mixed weight proportions of the butyl acrylate, N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, amino-modified emulsion, dipropylene glycol diacrylate, methyl methacrylate, ammonium dodecyl alcohol ether sulfate, EG emulsifier and ethyl acetate are respectively: 120-150 parts of butyl acrylate, 20-24 parts of N-(trimethylsilyl)-2-(trimethylsilyloxy)-4-pyrimidinamine, 80-100 parts of amino-modified emulsion, 10-16 parts of dipropylene glycol diacrylate, 20-25 parts of methyl methacrylate, 10-12 parts of ammonium dodecyl alcohol ether sulfate, 10-15 parts of EG emulsifier and 200-250 parts of ethyl acetate.
3. The environmentally friendly polyacrylate lithium battery adhesive tape according to claim 1, characterized in that: In the aqueous solution of ammonium persulfate and ammonium bicarbonate, the concentration of ammonium persulfate is 20-30 g / L, the concentration of ammonium bicarbonate is 12-16 g / L, and the solvent is water; the mass ratio of the mixture A of 1 / 5-1 / 6 mass and the aqueous solution of ammonium persulfate and ammonium bicarbonate is mixture A: aqueous solution of ammonium persulfate and ammonium bicarbonate = 10:2-3.
4. The environmentally friendly polyacrylate lithium battery adhesive tape according to claim 1, characterized in that: In the aqueous solution of sodium hydroxide, the concentration of sodium hydroxide is 10-15 g / L, and the solvent is water; the mass ratio of the N-aminoethyl-3-aminopropylmethyldimethoxysilane, epoxypropyltrimethoxysilane, the aqueous solution of sodium hydroxide and sodium dodecyl sulfate is N-aminoethyl-3-aminopropylmethyldimethoxysilane: epoxypropyltrimethoxysilane: the aqueous solution of sodium hydroxide: sodium dodecyl sulfate = 10:4-6:0.3-0.4:2-5.
5. The environmentally friendly polyacrylate lithium battery adhesive tape according to claim 1, characterized in that: The volume ratio of epichlorohydrin, acetone and water used to prepare the composite aqueous solution of epichlorohydrin and acetone is epichlorohydrin:acetone:water=4-6:50:50-60; the mass ratio of the composite aqueous solution of epichlorohydrin and acetone added to the mixture C is mixture C: composite aqueous solution of epichlorohydrin and acetone=1:1-2.
6. The environmentally friendly polyacrylate lithium battery adhesive tape according to claim 1, characterized in that: The mass ratio of the added mass of the tris(3-aminopropyl)amine to the mixture C is mixture C:tris(3-aminopropyl)amine=1:0.12-0.18.
Citation Information
Patent Citations
Cation-type quaternization organic fluorosilicon oil darkening finishing agent, and preparation method and application thereof
CN106012546A
Modified acrylate pressure-sensitive adhesive emulsion and preparation method thereof
CN107699167A
Lithium ion battery electrolyte and lithium ion battery prepared therefrom
CN108306048A
Preparation method of double-sided adhesive tape used for lithium battery
CN109868078A
Acrylic-coated silicon oxide-electroplated film and manufacturing method therefor
WO2022183554A1