A blast furnace ultra-high oxygen-enriched smelting method
By adjusting the combustion conditions of coke and pulverized coal in blast furnace smelting, the problem of pressure difference and poor air permeability after oxygen enrichment of the blast furnace is solved, efficient fuel utilization and low energy consumption smelting process are achieved, and the economic and technical indicators of the blast furnace are improved.
Patent Information
- Application Number
- CN202310055561.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-19
AI Technical Summary
In oxygen-enriched blast furnace smelting, the problems of increased pressure difference, poor air permeability and uneven development of gas flow caused by changes in the temperature field of the blast furnace limit the improvement of the economic and technical indicators of the blast furnace.
By limiting the index of coke entering the furnace, improving coke particle size uniformity, large proportion of center coking, controlling coke batch weight, adopting a low alkalinity slagging system and high blast kinetic energy air supply, and adjusting the oxygen enrichment rate and furnace gas volume index, Ensure the balance of blast furnace ventilation and hearth heat.
It achieves the goal of keeping the blast furnace running smoothly under high oxygen-rich conditions, reducing fuel consumption, increasing the temperature of slag and iron, enhancing the desulfurization capacity of acidic slag smelting, reducing the amount of iron slag per ton, reducing energy consumption and pollutant emissions, and improving the economic and technical indicators of the blast furnace.
Smart Images

Figure BDA0004060501270000041 
Figure BDA0004060501270000051 
Figure BDA0004060501270000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a blast furnace ultra-high oxygen-enriched smelting method. Background Art
[0002] The oxygen enrichment process is to add industrial oxygen before the hot air is sent into the blast furnace, so that the oxygen content of the blast exceeds the oxygen content of the atmosphere. At present, in order to improve quality and efficiency and reduce costs, the oxygen enrichment process is basically adopted in blast furnace ironmaking.
[0003] Nowadays, the oxygen enrichment rate in the wind of blast furnaces at home and abroad is generally controlled to be 1%-10%, that is, the total oxygen content is controlled at 23%-33%. There are the following problems in further increasing the oxygen enrichment rate:
[0004] (1) As the theoretical combustion temperature increases, the temperature field of the blast furnace body shows the problem of "cold on top and hot on the bottom", that is, the temperature of the blast furnace hearth is too high and the temperature of the upper part of the furnace body is too low, which leads to an increase in the blast furnace pressure difference, bringing serious impact on blast furnace smelting. This is the key problem in the development of ultra-high oxygen-enriched blast furnace smelting technology.
[0005] (2) The development of coal gas flow at the edge of the blast furnace and the increase in oxygen concentration and decrease in nitrogen content in the oxygen-enriched blast reduce the amount of coal gas produced per unit of pig iron smelting. If the smelting intensity remains unchanged, the vortex zone of the blast furnace tuyere will be reduced, resulting in the development of coal gas flow at the edge and the weakening of coal gas flow in the center, which will have a negative impact on the activity of the blast furnace hearth.
[0006] (3) The temperature zone for indirect reduction is highly reduced. Due to the change in temperature field, the residence time of the charge in the indirect reduction area is shortened after oxygen enrichment, which is not conducive to the indirect reduction.
[0007] In recent years, as steel mills have paid more and more attention to oxygen-enriched smelting in blast furnaces, people have also proposed methods for oxygen-enriched blast furnace smelting in blast furnaces: CN201810162301.2 discloses "a method for smelting vanadium-titanium magnetite in blast furnace using ultra-high oxygen-enriched blast", which increases the oxygen content in the blast furnace hot air to 26% to 41%, corresponding to a blast oxygen enrichment rate of 5% to 20%, thereby increasing the combustion rate of coal powder at the front end of the tuyere; improving the reduction potential of coal gas; optimizing the reduction, soft melting, dripping and slag-making process of vanadium-titanium magnetite in the blast furnace, improving the permeability of the blast furnace, and ensuring the stable and smooth production of the blast furnace; solving the problems of low coal ratio, high energy consumption, thick slag, poor permeability and difficulty in intensified smelting faced in the process of smelting vanadium-titanium magnetite by blast furnace process. By adding high-concentration oxygen to the blast furnace hot air to increase the oxygen content in the hot air, the coal injection ratio can be increased, the coke ratio can be reduced, the energy consumption of blast furnace ironmaking can be reduced, the smelting intensity can be increased, the blast furnace production can be stabilized, and the cost of blast furnace smelting of vanadium-titanium magnetite can be reduced.
[0008] However, the main principle of this method is to solve the problem of the deterioration of the blast furnace's smooth operation due to the increase in theoretical combustion temperature after oxygen enrichment of the blast furnace by large coal injection and high oxygen enrichment. The oxygen enrichment rate is limited by the amount of coal injection, and the maximum upper limit of the maximum oxygen enrichment rate is only 20%, which limits the further improvement of the blast furnace's economic and technical indicators. Summary of the invention
[0009] In order to overcome the shortcomings of the prior art, the present invention provides a blast furnace ultra-high oxygen-enriched smelting method, which solves the problem of increased pressure difference in the blast furnace caused by changes in the temperature field of the blast furnace after high-oxygen-enriched blasting, breaks through the current technical limitation that the oxygen enrichment rate of the blast furnace is generally controlled below 10%, and greatly improves the economic and technical indicators of the blast furnace.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] A blast furnace ultra-high oxygen-enriched smelting method, specifically as follows:
[0012] 1) Limit the coke index entering the furnace;
[0013] Specifically: coke M40 index>90%, M10 index<6%, CSR index>70%, ash content<11%.
[0014] 2) Improve the uniformity of coke particle size;
[0015] The proportion of particle size of coke entering the furnace of 40-60 mm is controlled to be greater than 45%, and the average particle size is controlled to be greater than 52 mm.
[0016] 3) Improve the combustion rate of pulverized coal; specifically: the volume percentage content of volatile matter in the injected pulverized coal is controlled at 30% to 40%.
[0017] 4) Large-scale center focus;
[0018] The material distribution method of center coking without a bell is adopted, and the amount of coke added in the center accounts for 50% to 60% of the batch weight of coke.
[0019] 5) Control the coke batch weight;
[0020] The batch weight of coke W is:
[0021] π·d 2 0.2 p 堆 / 3.8≤W 焦 ≤π·d 2 0.3 ρ 堆 / 3.8
[0022] Where: W 焦 is the coke batch weight, t;
[0023] d is the diameter of the blast furnace waist, m;
[0024] ρ堆 is the bulk density of coke, t / m 3 .
[0025] 6) Adopt low basicity slag making system; the binary basicity of slag is controlled at 0.2-0.4.
[0026] 7) Control the oxygen enrichment rate at 10% to 50%, that is, the volume percentage of oxygen in the blast is controlled at 29% to 52%.
[0027] 8) Control the gas volume index of the furnace to reduce the pressure difference in the furnace tuyere area;
[0028] When the oxygen volume percentage content in the blast is 40%≤≤50%, the gas volume index of the furnace is controlled at 48m / min≤<50m / min;
[0029] When the oxygen volume percentage content in the blast is 30%≤<40%, the gas volume index of the furnace should be controlled at 50m / min≤<51m / min;
[0030] When the oxygen volume percentage content in the blast is 20%≤<30%, the gas volume index of the furnace should be controlled at 51m / min≤<52m / min;
[0031] When the volume percentage of oxygen in the blast is 10%≤≤20%, the gas volume index of the furnace is controlled to be 52m / min≤54m / min.
[0032] 9) Control the blast kinetic energy to >160Kj / s.
[0033] 10) Control the amount of ore in the outermost ring of the chute to account for 20% to 30% of the weight of the ore batch.
[0034] Compared with the existing method, the beneficial effects of the present invention are:
[0035] 1) A blast furnace ultra-high oxygen-enriched smelting method is provided, which can ensure that the blast furnace can still run stably and smoothly after the blast oxygen enrichment rate is increased to 50%.
[0036] 2) After smelting in the blast furnace with ultra-high oxygen enrichment rate, the pulverized coal combustion rate before the tuyere can be effectively increased, thereby achieving the purpose of reducing the overall fuel consumption.
[0037] 3) This method overcomes the problem that in traditional high-oxygen-enriched smelting, large coal injection must be used to balance the theoretical combustion temperature before the tuyere to reduce the blast furnace pressure difference. Instead, it adopts an operating method to improve the permeability of the blast furnace, solving the problem of increased furnace pressure caused by increased theoretical combustion temperature after oxygen enrichment, and solving the problem of increased fuel ratio caused by reduced coal powder combustion rate during large coal injection.
[0038] 4) This method utilizes the increased heat of the furnace after ultra-high oxygen enrichment to increase the slag and iron temperature, solving the problems of weak desulfurization capacity and poor slag fluidity in acidic slag smelting. At the same time, acidic slag smelting can reduce the amount of alkaline solvent entering the furnace and the amount of slag per ton of iron, effectively reducing the blast furnace pressure difference while comprehensively improving the economic and technical indicators of the blast furnace.
[0039] 5) The use of acidic slag smelting can effectively reduce the accumulation of harmful elements such as alkali metals in the furnace and extend the life of the blast furnace.
[0040] 6) Through acidic slag smelting, the amount of iron slag per ton can be greatly reduced, which is beneficial to energy conservation and emission reduction.
[0041] 7) Acidic slag smelting can reduce the consumption of iron ore per ton, which is beneficial to reducing the cost per ton of iron.
[0042] 8) Through ultra-high oxygen-enriched smelting, the heat of the furnace can be effectively increased and the temperature of the molten iron can be increased, which is beneficial to increase the proportion of scrap steel in the subsequent steelmaking process and reduce steelmaking costs and pollutant emissions.
[0043] The present invention solves the problem of poor air permeability of the blast furnace after ultra-high oxygen enrichment by means of large-proportion central coking, controlling the upper and lower limits of the coke batch weight, improving the uniformity of the coke particle size entering the furnace, and limiting the upper limit of the furnace belly gas volume index. It also solves the problem of low furnace top temperature and the condensation of water vapor in the coal gas that easily blocks the bag dust removal system. At the same time, the high kinetic energy of the blast air supply system solves the problem of the development of the edge coal gas flow after oxygen enrichment. The most important thing is to use the characteristics of super-high oxygen enrichment smelting furnace cylinder overheating and sufficient heat to solve the problems of weak desulfurization ability and poor slag fluidity in acidic slag smelting, and acidic slag smelting can reduce the amount of alkaline solvent entering the furnace, that is, improve the furnace grade, significantly reduce the amount of slag per ton of iron, which is beneficial to energy saving and consumption reduction in the blast furnace smelting process. DETAILED DESCRIPTION
[0044] The present invention discloses a blast furnace ultra-high oxygen-enriched smelting method. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0045] A method for smelting blast furnace with ultra-high oxygen enrichment, which improves the production efficiency of blast furnace by increasing the concentration of O2 in blast air through ultra-high oxygen enrichment smelting, and can also increase the concentration of CO in coal gas to promote indirect reduction, so as to achieve the purpose of reducing solid combustion; in order to further solve the problem of increased fuel consumption caused by overheating of the lower part of the blast furnace and poor permeability due to the change of the temperature field of the blast furnace to "cold on the top and hot on the bottom" after excessive oxygen enrichment, and the reduction of the indirect reduction area of the blast furnace due to overcooling of the upper part of the blast furnace, the method is first proposed to use large-proportion central coking, control the lower limit of coke batch weight, control the uniformity of blast furnace coke particle size and limit the upper limit of the furnace gas volume index; at the same time, the problem of excess edge coal gas flow and weakened center coal gas flow due to the reduction of coal gas volume after oxygen enrichment in the blast furnace is solved by high blast kinetic energy air supply. The most important thing is that the sufficient heat of the furnace cylinder of ultra-high oxygen enrichment smelting solves the problems of weak desulfurization ability and poor slag fluidity of acidic slag smelting, and acidic slag smelting can reduce the amount of alkaline solvent entering the furnace, that is, reduce the amount of ton of iron slag, and also improve the furnace grade.
[0046] The details are as follows:
[0047] 1. Improve the permeability of the blast furnace by limiting the coke index entering the furnace, specifically: coke M40 index>90%, M10 index<6%, CSR index>70%, ash content<11%.
[0048] 2. Ensure the air permeability and top temperature of the blast furnace by improving the uniformity of coke particle size, specifically: control the proportion of coke particles of 40-60 mm entering the furnace to be greater than 45%, and the average particle size to be greater than 52 mm.
[0049] 3. Improve the combustion rate of pulverized coal and control the volatile matter content in the injected pulverized coal at 30% to 40%.
[0050] 4. Improve the permeability and top temperature of the blast furnace by adding coke in large proportion at the center, and adopt the distribution method of adding coke in the center without charging bell. The amount of coke added in the center accounts for 50% to 60% of the coke batch weight.
[0051] 5. Control the coke batch weight. The coke batch weight Wcoke is:
[0052]
[0053] In the formula: Wcoal is the coke batch weight, t; d is the blast furnace waist diameter, m; ρpile is the coke bulk density, t / m 3 .
[0054] 6. Use low-alkalinity slag-making system to reduce the amount of lime entering the furnace and thus reduce the amount of slag to improve the permeability of the blast furnace. The binary alkalinity of the slag is controlled at 0.2-0.4.
[0055] 7. Control the oxygen enrichment rate in the blast within a reasonable range to ensure the fluidity and desulfurization performance of the acidic slag in the furnace. Specifically: control the oxygen enrichment rate in the blast within 10-50%, that is, the volume percentage of oxygen in the blast is controlled within 29%-52%, to ensure the fluidity and desulfurization performance of the acidic slag in the furnace.
[0056] 8. Reduce the pressure difference in the furnace tuyere area by controlling the furnace gas volume index, specifically:
[0057] When the volume percentage of oxygen in the blast is 40% to 50%, the gas volume index of the furnace is controlled to be 48-50m / min;
[0058] When the volume percentage of oxygen in the blast is 30-40%, the gas volume index of the furnace is controlled to be 50-51m / min;
[0059] When the volume percentage of oxygen in the blast is 20-30%, the gas volume index of the furnace is controlled to be 51-52m / min;
[0060] When the volume percentage of oxygen in the blast is 10-20%, the furnace gas volume index is controlled to be 52-54m / min.
[0061] 9. Control the blast kinetic energy to >160Kj / s to promote the development of central gas flow.
[0062] 10. The amount of ore distributed in the outermost ring of the chute accounts for 20% to 30% of the weight of the ore batch, which inhibits the development of marginal coal gas flow.
[0063] [Example]
[0064] Before ultra-high oxygen enrichment:
[0065] The oxygen enrichment rate of the blast is 3.3% (the oxygen content in the blast is 25.1%): at a certain altitude of 3200m 3 The blast furnace uses 75% sintered ore and 25% pelletized ore as raw materials; coke (metallurgical properties and particle size indicators are shown in Table 1 and Table 2) and ore (composition is shown in Table 3) are added to the blast furnace by the blast furnace top distribution equipment; oxygen is directly added from the cold air duct in front of the blower, and is blown into the blast furnace after being heated by the heating furnace. Coal powder is sprayed into the blast furnace from the coal gun at the front end of the tuyere (coal powder injection indicators are shown in Table 4), and the blast furnace operating parameters are as follows (blast furnace distribution matrix is shown in Table 5, blast furnace air supply parameters are shown in Table 6, and slag composition is shown in Table 7):
[0066] Table 1 Coke performance indicators (wt%)
[0067] M40 M10 CSR CRI Ash 88.2 7.2 65.6 23.1 12.4
[0068] Table 2 Coke particle size composition (%)
[0069] <25mm 25-40mm 40-60mm 60-80mm >80mm Average particle size, mm 3.8 30.8 43.8 18.0 3.6 48.6
[0070] Table 3 Chemical composition of iron ore (wt%)
[0071] Element TFe FeO CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> S R Proportion Sintered ore 50.64 9.05 11.74 5.65 1.1 1.05 0.025 2.053 75 Pelletized Ore 60.2 0.25 0.25 6.17 1.9 0.29 0.01 0.05 25
[0072] (Iron ore consumption per ton is 1.816t / t, and the average iron ore grade entering the furnace is 53.03%)
[0073] Table 4 Coal injection composition ratio (wt%)
[0074]
[0075]
[0076] Table 5 Blast furnace distribution matrix
[0077] Gear 10 9 8 7 6 5 4 3 2 1 angle 41.0 39.0 36.7 34.2 31.5 28.6 25.7 22.2 15.2 13.0 K Big 1 3 2 2 2 J University 3 3 2 2 2 2
[0078] (of which the batch weight of coke is 16.6t and the batch weight of ore is 88.2t)
[0079] Table 6 Blast furnace air supply parameters
[0080] Oxygen enrichment Air volume Wind temperature Blast humidity Blowing energy Bosh gas volume index <![CDATA[m 3 / h]]> <![CDATA[m 3 / min]]> ℃ <![CDATA[g / m 3 ]]> Kj / s <![CDATA[m 3 / min]]> 15000 6000 1150 0.02 123 58.5
[0081] Table 7 Blast furnace slag composition (wt%)
[0082]
[0083] The economic and technical indicators of blast furnace are as follows (see Table 8)
[0084] Table 8 Economic and technical indicators of blast furnace
[0085] Focal Ratio Jiao Dingbi Coal ratio Fuel ratio Nissan Slag volume tons of iron Kg / t Kg / t Kg / t Kg / t t / d Kg / t 348 57.4 169.4 574.8 7200 365.6
[0086] After ultra-high oxygen enrichment:
[0087] Embodiment 1:
[0088] The oxygen enrichment rate of the blast is 10.6% (the oxygen content in the blast is 30.9%): at a certain altitude of 3200m 3 The blast furnace uses 75% sintered ore and 25% pelletized ore as raw materials; coke and ore are added to the blast furnace through the blast furnace top distribution equipment; oxygen is directly added through the cold air duct in front of the blower, and is blown into the blast furnace after being heated by the heating furnace, and coal powder is sprayed into the blast furnace through the coal gun at the front end of the tuyere. The blast furnace operating parameters are as follows:
[0089] By increasing the coking time of the coke oven or increasing the proportion of coking coal, the metallurgical performance indicators and average particle size of coke are improved (see Table 9 and Table 10).
[0090] Table 9 Coke performance index (wt%)
[0091] M40 M10 CSR CRI Ash 90.2 5.2 71.6 20.2 10.4
[0092] Table 10 Coke particle size composition (%)
[0093] <25mm 25-40mm 40-60mm 60-80mm >80mm Average particle size mm 1.4 22.3 47.0 25.6 3.7 52.5
[0094] By reducing the proportion of lime in the sintering process, lowering the alkalinity of the sintered ore, and improving the comprehensive grade of iron ore entering the furnace (see Table 11), under the condition that the iron ore powder remains unchanged during the sintering process, the comprehensive grade of iron ore entering the furnace is increased from the previous 53.03% to 55.78% after oxygen enrichment, and the comprehensive grade entering the furnace is increased by 2.7 percentage points, the consumption per ton of iron ore is reduced by 0.104t, and the cost of raw materials per ton of iron is reduced by 60.6 yuan / t.
[0095] Table 11 Chemical composition of iron ore (wt%)
[0096] Element TFe FeO CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> S R Proportion Sintered ore 54.3 9.1 2.18 6.258 1.1 1.12 0.025 0.3484 75 Pelletized Ore 60.2 0.25 0.25 6.17 1.9 0.29 0.01 0.05 25
[0097] (Iron ore consumption per ton is 1.712t / t, and the average iron ore grade entering the furnace is 55.78%)
[0098] Increase the proportion of bituminous coal, reduce the proportion of anthracite, and control the volatile matter to 31% (see Table 12).
[0099] Table 12 Composition ratio of PCI (wt%)
[0100] Product Name Ash Volatile Matter sulfur Moisture Fixed Carbon Ratio Shenhua 6.06 34.06 0.25 12.20 59.88 90.0% put down 10.80 6.45 0.93 9.55 82.75 5.0% Russia 6.58 3.08 0.35 14.70 90.34 0.0% Coking dust removal 12.88 1.18 0.80 10.00 85.94 5.0% Prediction Components 6.64 31.04 0.31 11.96 62.33 100.00%
[0101] By adjusting the distribution matrix, the pressure edge and center coke distribution system (see Table 13) was adopted. The amount of ore distributed in the outermost 10th ring of the chute accounted for 27.3% of the ore batch weight. Seven rings of coke were distributed in the center of the throat, accounting for 53.8% of the coke batch weight. The diameter of the blast furnace waist is 13.7m. In order to ensure that the coke layer thickness at the furnace waist is within the range of 0.2-0.3m, the coke batch weight is 16.6t as before, but due to the significant reduction in coke ratio, the ore batch is increased to 98.9t.
[0102] Table 13 Blast furnace distribution matrix
[0103] Gear 10 9 8 7 6 5 4 3 2 1 angle 41.0 39.0 36.7 34.2 31.5 28.6 25.7 22.2 15.2 13.0 K Big 3 2 2 2 2 J University 1 1 1 2 2 7
[0104] (of which the batch weight of coke is 16.6t and the batch weight of ore is 98.9t)
[0105] Oxygen is directly added from the cold air duct in front of the blower, and then blown into the blast furnace after being heated by the heating furnace. The blast furnace operating parameters are as follows (see Table 14). The oxygen flow rate of the blast furnace is increased to 36000m 3 / h, the oxygen enrichment rate was increased to 10.6%. To promote the development of the central coal gas flow, the blast kinetic energy was increased to 163Kj / s. At the same time, to ensure the air permeability of the lower part of the furnace body, the blast flow rate was reduced to 4500m3 / min, the furnace gas volume index is reduced to 52.6m / min.
[0106] Table 14 Blast furnace air supply parameters
[0107] Oxygen enrichment Air volume Wind temperature Blast humidity Blowing energy Bosh gas volume index <![CDATA[m 3 / h]]> <![CDATA[m 3 / min]]> ℃ <![CDATA[g / m 3 ]]> Kj / s m / min 36000 4500 1152 0.02 163 52.6
[0108] By reducing the basicity of sintered ore, the binary basicity of slag is reduced to 0.22, and the slag composition is as follows (see Table 15)
[0109] Table 15 Blast furnace slag composition (wt%)
[0110]
[0111] The economic and technical indicators of blast furnace are as follows (see Table 16)
[0112] Although the blast air volume is reduced, the oxygen enrichment rate is significantly increased, and the blast furnace output is also increased. The average daily output of the blast furnace reaches 7600t / d, an increase of 400t. In addition, due to the improvement of the furnace grade, the blast furnace slag per ton is reduced by 121.3kg / t, and the fuel ratio is also significantly reduced to 522kg / t. Compared with the ultra-high oxygen enrichment, it is reduced by 52.8kg / t.
[0113] Table 16 Economic and technical indicators of blast furnace
[0114] Focal Ratio Jiao Dingbi Coal ratio Fuel ratio Nissan Slag volume Kg / t Kg / t Kg / t Kg / t t / d Kg / t 301 50.4 170.6 522 7600 244.3
[0115] Embodiment 2:
[0116] The oxygen enrichment rate of the blast is 45.8% (the oxygen content in the blast is 49.9%): at a certain altitude of 3200m 3 The blast furnace uses 80% sintered ore and 20% pelletized ore as raw materials; coke and ore are added to the blast furnace through the blast furnace top distribution equipment; oxygen is directly added through the cold air duct in front of the blower, and is blown into the blast furnace after being heated by the heating furnace, and coal powder is sprayed into the blast furnace through the coal gun at the front end of the tuyere. The blast furnace operating parameters are as follows:
[0117] By increasing the coking time of the coke oven or increasing the proportion of coking coal, the metallurgical performance indicators and average particle size of coke are improved (see Table 17 and Table 18).
[0118] Table 17 Coke performance index (wt%)
[0119] M40 M10 CSR CRI Ash 90.3 5.6 70.6 20.1 10.2
[0120] Table 18 Coke particle size composition (%)
[0121] <25mm 25-40mm 40-60mm 60-80mm >80mm Average particle size, mm 1.8 22.8 49.8 20.0 5.6 52.1
[0122] By reducing the proportion of lime in the sintering process, lowering the alkalinity of the sintered ore, and improving the comprehensive grade of iron ore entering the furnace (see Table 19), under the condition that the iron ore powder remains unchanged during the sintering process, the comprehensive grade of iron ore entering the furnace is increased from the previous 53.03% to 55.74% after oxygen enrichment, and the comprehensive grade entering the furnace is increased by 2.7 percentage points, the consumption per ton of iron ore is reduced by 0.115t, and the cost of raw materials per ton of iron is reduced by 61.2 yuan / t.
[0123] Table 19 Chemical composition of iron ore (wt%)
[0124] Element TFe FeO CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> S R Proportion Sintered ore 54.6 9.2 2.19 6.558 1.11 1.09 0.02 0.3339 80 Pelletized Ore 60.3 0.23 0.25 6.37 1.8 0.21 0.01 0.039 20
[0125] (Iron ore consumption per ton is 1.701t / t, and the average iron ore grade entering the furnace is 55.74%)
[0126] Increase the proportion of bituminous coal, reduce the proportion of anthracite, and control the volatile matter to 32.42% (see Table 20).
[0127] Table 20 PCI composition ratio (wt%)
[0128] Product Name Ash Volatile Matter sulfur Moisture Fixed Carbon Ratio Shenhua 6.06 34.06 0.25 12.20 59.88 95.0% put down 10.80 6.45 0.93 9.55 82.75 0.0% Russia 6.58 3.08 0.35 14.70 90.34 0.0% Coking dust removal 12.88 1.18 0.80 10.00 85.94 5.0% Prediction Components 6.40 32.42 0.28 12.09 61.18 100%
[0129] By adjusting the distribution matrix, the pressure edge and center coke distribution system (see Table 21) was adopted. The amount of ore distributed in the outermost 10th ring of the chute accounted for 27.3% of the ore batch weight. Seven rings of coke were distributed in the center of the throat, accounting for 53.8% of the coke batch weight. The diameter of the blast furnace waist is 13.7m. In order to ensure that the coke layer thickness at the waist is within the range of 0.2-0.3m, the coke batch weight is 16.5t as before, but due to the significant reduction in coke ratio, the ore batch is increased to 98.7t.
[0130] Table 21 Blast furnace distribution matrix
[0131] Gear 10 9 8 7 6 5 4 3 2 1 angle 41.0 39.0 36.7 34.2 31.5 28.6 25.7 22.2 15.2 13.0 K Big 3 2 2 2 2 J University 1 1 1 2 2 7
[0132] (of which the batch weight of coke is 16.5t and the batch weight of ore is 98.7t)
[0133] Oxygen is directly added from the cold air duct in front of the blower, and then blown into the blast furnace after being heated by the heating furnace. The blast furnace operating parameters are as follows (see Table 22). The oxygen flow rate of the blast furnace is increased to 90,000 m 3 / h, the oxygen enrichment rate was increased to 45.8%. To promote the development of the central coal gas flow, the blast kinetic energy was increased to 169Kj / s. At the same time, to ensure the air permeability of the lower part of the furnace body, the blast flow rate was reduced to 2600m 3 / min, the furnace gas volume index is reduced to 48.9m / min.
[0134] Table 22 Blast furnace air supply parameters
[0135] Oxygen enrichment Air volume Wind temperature Blast humidity Blowing energy Bosh gas volume index <![CDATA[m 3 / h]]> <![CDATA[m 3 / min]]> ℃ <![CDATA[g / m 3 ]]> Kj / s m / min 90000 2600 1157 0.02 169 48.9
[0136] By reducing the basicity of sintered ore, the binary basicity of slag is reduced to, and the slag composition is as follows (see Table 23)
[0137] Table 23 Blast furnace slag composition (wt%)
[0138]
[0139] The economic and technical indicators of blast furnace are as follows (see Table 24)
[0140] Although the blast air volume is reduced, the oxygen enrichment rate is significantly increased, and the blast furnace output is also increased. The average daily output of the blast furnace reaches 7500t / d, an increase of 300t. In addition, due to the improvement of the furnace grade, the blast furnace slag per ton is reduced by 118.3kg / t, and the fuel ratio is also significantly reduced to 509.8kg / t. Compared with the ultra-high oxygen enrichment, it is reduced by 65kg / t.
[0141] Table 24 Economic and technical indicators of blast furnace
[0142] Focal Ratio Jiao Dingbi Coal ratio Fuel ratio Nissan Slag volume Kg / t Kg / t Kg / t Kg / t t / d Kg / t 291 40.2 178.6 509.8 7500 247.3
[0143] Embodiment 3:
[0144] The oxygen enrichment rate of the blast is 27.3% (the oxygen content in the blast is 41.2%): at a certain altitude of 3200m 3 The blast furnace uses 75% sintered ore and 25% pelletized ore as raw materials; coke and ore are added to the blast furnace through the blast furnace top distribution equipment; oxygen is directly added through the cold air duct in front of the blower, and is blown into the blast furnace after being heated by the heating furnace, and coal powder is sprayed into the blast furnace through the coal gun at the front end of the tuyere. The blast furnace operating parameters are as follows:
[0145] By increasing the coking time of the coke oven or increasing the proportion of coking coal, the metallurgical performance indicators and average particle size of coke are improved (see Tables 25 and 26).
[0146] Table 25 Coke performance index (wt%)
[0147] M40 M10 CSR CRI Ash 91.3 5.0 72.2 19.1 10.1
[0148] Table 26 Coke particle size composition (%)
[0149] <25mm 25-40mm 40-60mm 60-80mm >80mm Average particle size mm 1.0 23.4 50.9 18.9 5.8 52.2
[0150] By reducing the proportion of lime in the sintering process, lowering the alkalinity of the sintered ore, and improving the comprehensive grade of iron ore entering the furnace (see Table 27), under the condition that the iron ore powder remains unchanged during the sintering process, the comprehensive grade of iron ore entering the furnace is increased from the previous 53.03% to 55.46% after oxygen enrichment, and the comprehensive grade entering the furnace is increased by 2.4 percentage points, the consumption per ton of iron ore is reduced by 0.95t, and the cost of raw materials per ton of iron is reduced by 52.6 yuan / t.
[0151] Table 27 Chemical composition of iron ore (wt%)
[0152] Element TFe FeO CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> S R Proportion Sintered ore 54.6 9.2 2.19 6.558 1.11 1.09 0.02 0.339 85 Pelletized Ore 60.3 0.23 0.25 6.37 1.8 0.21 0.01 0.039 15
[0153] (Iron ore consumption per ton is 1.721t / t, and the average iron ore grade entering the furnace is 55.46%)
[0154] Increase the proportion of bituminous coal, reduce the proportion of anthracite, and control the volatile matter to 32.51% (see Table 28).
[0155] Table 28 Composition ratio of PCI coal (wt%)
[0156] Product Name Ash Volatile Matter sulfur Moisture Fixed Carbon Ratio Shenhua 6.06 34.06 0.25 12.20 59.88 95.0% put down 10.80 6.45 0.93 9.55 82.75 0.0% Russia 6.58 3.08 0.35 14.70 90.34 5.0% Coking dust removal 12.88 1.18 0.80 10.00 85.94 0.0% Prediction Components 6.09 32.51 0.26 12.33 61.40 100%
[0157] By adjusting the distribution matrix, the pressure edge and center coke distribution system (see Table 29) was adopted. The amount of ore distributed in the outermost 10th ring of the chute accounted for 27.3% of the ore batch weight. Seven rings of coke were distributed in the center of the throat, accounting for 53.8% of the coke batch weight. The diameter of the blast furnace waist is 13.7m. In order to ensure that the coke layer thickness at the waist is within the range of 0.2-0.3m, the coke batch weight is 16.5t as before, but due to the significant reduction in coke ratio, the ore batch is increased to 98.7t.
[0158] Table 29 Blast furnace distribution matrix
[0159] Gear 10 9 8 7 6 5 4 3 2 1 angle 41.0 39.0 36.7 34.2 31.5 28.6 25.7 22.2 15.2 13.0 K Big 3 2 2 2 2 J University 1 1 1 2 2 7
[0160] (of which the batch weight of coke is 17.5t and the batch weight of ore is 103.7t)
[0161] Oxygen is directly added from the cold air duct in front of the blower, and then blown into the blast furnace after being heated by the heating furnace. The blast furnace operating parameters are as follows (see Table 30). The oxygen flow rate of the blast furnace is increased to 70,000 m 3 / h, the oxygen enrichment rate was increased to 45.8%, and the blast kinetic energy was increased to 173Kj / s to promote the development of the central coal gas flow. At the same time, in order to ensure the air permeability of the lower part of the furnace body, the blast flow rate was reduced to 3400m 3 / min, the furnace gas volume index is reduced to 51.2m / min.
[0162] Table 30 Blast furnace air supply parameters
[0163] Oxygen enrichment Air volume Wind temperature Blast humidity Blowing energy Bosh gas volume index <![CDATA[m 3 / h]]> <![CDATA[m 3 / min]]> ℃ <![CDATA[g / m 3 ]]> Kj / s m / min 70000 3400 1202 0.02 173 51.2
[0164] By reducing the basicity of sintered ore, the binary basicity of slag is reduced to, and the slag composition is as follows (see Table 31)
[0165] Table 31 Blast furnace slag composition (wt%)
[0166]
[0167] The economic and technical indicators of blast furnace are as follows (see Table 32)
[0168] Although the blast air volume is reduced, the oxygen enrichment rate is significantly increased, and the blast furnace output is also increased. The average daily output of the blast furnace reaches 7400t / d, an increase of 200t. In addition, due to the improvement of the furnace grade, the blast furnace slag per ton is reduced by 111.5kg / t, and the fuel ratio is also significantly reduced to 530.2kg / t, which is 44.8kg / t lower than before the ultra-high oxygen enrichment.
[0169] Table 32 Economic and Technical Indicators of Blast Furnace
[0170] Focal Ratio Jiao Dingbi Coal ratio Fuel ratio Nissan Slag volume Kg / t Kg / t Kg / t Kg / t t / d Kg / t 307 50.6 172.6 530.2 7400 254.1
[0171] The present invention solves the problem of poor air permeability of the blast furnace after ultra-high oxygen enrichment by means of large-proportion central coking, controlling the upper and lower limits of the coke batch weight, improving the uniformity of the coke particle size entering the furnace, and limiting the upper limit of the furnace belly gas volume index. It also solves the problem of low furnace top temperature and the condensation of water vapor in the coal gas that easily blocks the bag dust removal system. At the same time, the high kinetic energy of the blast air supply system solves the problem of the development of the edge coal gas flow after oxygen enrichment. The most important thing is to use the characteristics of super-high oxygen enrichment smelting furnace cylinder overheating and sufficient heat to solve the problems of weak desulfurization ability and poor slag fluidity in acidic slag smelting, and acidic slag smelting can reduce the amount of alkaline solvent entering the furnace, that is, improve the furnace grade, significantly reduce the amount of slag per ton of iron, which is beneficial to energy saving and consumption reduction in the blast furnace smelting process.
[0172] The invention solves the problem of increased pressure difference in the blast furnace due to temperature field change after high oxygen-enriched blasting, breaks through the technical limitation that the oxygen enrichment rate of the blast furnace is generally controlled below 10%, and greatly improves the economic and technical indicators of the blast furnace.
[0173] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A blast furnace ultra-high oxygen-enriched smelting method, It is characterized in that The details are as follows: 1) Limit the coke index entering the furnace; 2) Improve the uniformity of coke particle size; Control the proportion of coke particles between 40 and 60 mm entering the furnace to be greater than 45%, and the average particle size to be greater than 52 mm; 3) Improve the combustion rate of pulverized coal; 4) Large-scale center focus; The material distribution method of center coking without a bell is adopted, and the amount of coke added in the center accounts for 50%~60% of the coke batch weight; 5) Control the coke batch weight; The batch weight of coke W is: p·d 2 ·0.2·r 堆 / 3.8 ≤ W 焦 ≤ π d 2 ·0.3·r 堆 / 3.8; Where: W 焦 is the coke batch weight, t; d is the diameter of the blast furnace waist, m; ρ 堆 is the bulk density of coke, t / m 3 ; 6) Adopt low basicity slagging system; 7) Control the oxygen enrichment rate to 10%~50%, that is, the volume percentage of oxygen in the blast is controlled at 29%~52%; 8) Control the gas volume index of the furnace to reduce the pressure difference in the furnace tuyere area; When the oxygen enrichment rate is 40%≤≤50%, the gas volume index of the furnace should be controlled to be 48m / min≤<50m / min; When the oxygen enrichment rate is 30%≤<40%, control the gas volume index of the furnace to be 50m / min≤<51m / min; When the oxygen enrichment rate is 20%≤<30%, the gas volume index of the furnace should be controlled to be 51m / min≤<52m / min; When the oxygen enrichment rate is 10%≤<20%, the gas volume index of the furnace should be controlled at 52m / min≤≤54m / min; 9) Control the blast kinetic energy>160KJ / s; 10) Control the amount of ore in the outermost ring of the chute to account for 20%~30% of the weight of the ore batch.
2. A blast furnace ultra-high oxygen-enriched smelting method according to claim 1, It is characterized in that The step 1) limits the coke index entering the furnace to improve the blast furnace permeability, specifically: coke M40 index>90%, M10 index<6%, CSR index>70%, ash content<11%.
3. A blast furnace ultra-high oxygen-enriched smelting method according to claim 1, It is characterized in that The step 3) improves the combustion rate of the pulverized coal, specifically, the volume percentage content of the volatile matter in the injected pulverized coal is controlled at 30% to 40%.