Method for preparing aluminum foil material for battery with low-density distributed second phase particles

Optimizing the alloy ratio and process flow of aluminum foil materials through green short-process casting and rolling method, solving the problem of insufficient molding performance of lithium battery soft bag materials, achieving the improvement of high-deep burst performance and mechanical properties, and is suitable for new energy lithium-ion soft bags Deep-draining of the battery.

CN116043070BActive Publication Date: 2024-11-08JIANGSU DINGSHENG NEW MATERIAL JOINT STOCK CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310024356.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-08
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The existing aluminum foil material has insufficient molding performance in lithium battery soft-pack materials, resulting in low cup burst value, which cannot meet the needs of new energy lithium batteries for high-deep and long-term life.

Method used

Using green short-process casting and rolling method, the aluminum foil material with low-density distribution of second phase particles is prepared through precise alloying elements, online aluminum melt mass treatment and filtration technology, and cold rolling process heat treatment process optimization, and the material's deep-draining performance is improved. and mechanical properties.

Benefits of technology

It has achieved high-deep digging performance improvement of aluminum foil materials, excellent mechanical properties, Vickers hardness is 50-60Hv, tensile strength is 150-170Mpa, elongation is ≥3.0%, and reduced production costs and energy consumption, suitable for new energy lithium ion Deep-drain processing of soft-pack batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043070B_ABST
    Figure CN116043070B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an aluminum foil material for a battery with low-density distribution of second-phase particles. The preparation method is produced using a green short-process casting and rolling method. By optimizing the precise proportion of alloy elements, online aluminum melt quality treatment and filtering technology, and cold rolling process heat treatment process, the aluminum foil material for new energy lithium-ion soft-pack batteries can meet the high deep drawing and lithium battery service characteristics. At the same time, the aluminum foil material for new energy lithium-ion soft-pack batteries of the invention has excellent mechanical properties, which is convenient for subsequent deep drawing without cracks. The raw material performance Vickers hardness is 50-60Hv, the tensile strength is 150-170Mpa, and the elongation is ≥3.0%. The excellent mechanical properties can improve the subsequent processing performance of the aluminum foil material for new energy lithium-ion soft-pack batteries. The present invention adopts a casting-cold rolling process to replace the conventional hot rolling-cold rolling process, which has the advantages of short process and low production cost, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an aluminum foil material for a battery with low-density distributed second-phase particles. Background Art

[0002] With the development of the battery industry, end-user groups have increasingly stringent requirements on the use of soft-pack lithium batteries, and require higher safety performance, longer battery life and battery cell capacity.

[0003] Based on various factors, manufacturers of soft-pack lithium batteries try to increase the space used to store battery cells without increasing the thickness of the battery soft-pack material. Therefore, they hope that the soft-pack material will have better molding properties to meet increasingly stringent practical requirements.

[0004] The aluminum foil manufacturing end often uses the cupping value of the aluminum foil material to measure this kind of forming performance. The larger the cupping value, the better the material forming performance. The smaller the cupping value, the poorer the material processing performance and the less suitable it is for lithium battery soft pack materials. The metallographic photo analysis of the material shows that the deep drawing performance of the material is closely related to the size and distribution of the second phase particles in the metallographic structure. Reasonable control of the size and distribution of the second phase particles can effectively improve the deep drawing performance of the material.

[0005] Therefore, there is an urgent need for an aluminum foil production process that can reduce the distribution of second phase particles to obtain aluminum foil materials with better cupping value to match the development trend of new energy lithium batteries. Summary of the invention

[0006] The purpose of the present invention is to solve the above shortcomings of the prior art and propose a method for preparing a battery aluminum foil material with low-density distributed second phase particles.

[0007] In order to overcome the above-mentioned defects, a method for preparing a raw material of aluminum foil material for new energy lithium-ion soft-pack batteries with low-density distribution second-phase particles is provided. The raw material is produced by a green short-process casting and rolling method. The aluminum foil material for new energy lithium-ion soft-pack batteries can meet the high deep drawing and lithium battery service characteristics by accurately proportioning alloy elements, online aluminum melt quality treatment and filtration technology, and cold rolling process heat treatment process optimization. At the same time, the aluminum foil material for new energy lithium-ion soft-pack batteries of the present invention has excellent mechanical properties, which is convenient for subsequent deep drawing without cracks. The raw material performance Vickers hardness is 50-60Hv, the tensile strength is 150-170Mpa, and the elongation is ≥3.0%. The excellent mechanical properties can improve the subsequent processing performance of the aluminum foil material for new energy lithium-ion soft-pack batteries. The present invention adopts a casting-cold rolling process to replace the conventional hot rolling-cold rolling process, which has the advantages of short process and low production cost, and has good application prospects.

[0008] A method for preparing a raw material of aluminum foil material for new energy lithium-ion soft-pack batteries with low-density distributed second-phase particles, comprising the following steps:

[0009] (1) Preparation of alloy composition: Alloy elements are proportioned according to the following formula: Fe content is 1.4-1.5%, Si content is 0.03-0.05%, Ti content is 0.01-0.02%, Cu element is 0.002-0.0035%, and the balance is aluminum, wherein the sum of the weight percentages of Fe, Si, Cu, Ti and Al is 100%.

[0010] (2) Melting: Fe and Si elements are added in the form of intermediate alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before adding to the melting furnace. After 1 / 3 of the aluminum liquid is flattened, Si and Fe elements are added to the melting furnace, and 3-4kg / t of aluminum liquid is added to prevent the aluminum liquid from further oxidation and slag formation. The refining process is carried out for 4-5 hours, and the refining agent is added at a ratio of 0.8-1.2kg / t of aluminum liquid. At the same time, argon gas is introduced for powder blowing refining, and the refining is controlled for 30 minutes; after the "return" and "W" type operations are completed, argon gas is introduced into the melting furnace to maintain positive pressure in the furnace and keep it still for 1 hour. When no slag is visible on the surface of the aluminum liquid, the furnace pouring process is carried out.

[0011] (3) Online multi-stage composite filtration technology: The aluminum liquid treated in step (2) is passed into a filter box, which adopts a combination of tubular and plate filtration technology. The first-stage filter plate has a mesh number of 50 Ppi, the temperature in the insulation box is controlled at 725-730°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 1:1) is passed into the filter box; the second-stage filter plate has a mesh number of 70 Ppi, the temperature in the insulation box is controlled at 720-725°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 2:1) is passed into the filter box; the third-stage filter plate is a tubular filter RC grade, the mesh number is 100 Ppi, the temperature in the insulation box is controlled at 710-715°C, and argon is passed into the filter box; then the aluminum liquid passes through a casting and rolling mill to obtain a cast-rolled coil billet with a thickness of 8.0-8.5 mm. The casting and rolling zone has a length of 45-52 mm, an opening of 13 mm, and a liquid level fluctuation control of 2-4 mm.

[0012] (4) Heat treatment technology: The cast-rolled coil obtained in step (3) is rolled for one pass and then heat treated. The outer ring is welded, the steel strip is tightened on the plate surface, and homogenization annealing is carried out in a high-temperature annealing furnace, and the furnace gas temperature is kept at 240°C for 10 hours. Then the temperature is raised to the target heating temperature of 500-560°C at 1-1.5°C / min, and the temperature is kept for 5-8 hours after reaching the target heating temperature. Then the furnace gas temperature is cooled at 3-4°C / min. When the furnace gas temperature reaches 350°C, it is immediately taken out of the furnace and air-cooled to obtain a semi-finished aluminum coil.

[0013] (5) Cold rolling and secondary heat treatment: The semi-finished product obtained in step (4) is rolled to 0.5-1.0 mm, wherein the crown of the cold rolling mill support roller is controlled at 0.03 mm, the roughness Ra value is 0.5-0.7 μm, the online plate shape is controlled at 10-12I during rolling, the oil temperature is controlled at 33-37°C, the oil nozzle flow rate is controlled at 40-45%, and the oil acid value is controlled at 0.3-0.4 mgKOH / g. The semi-finished product 0.5-1.0 mm is transferred to the annealing furnace for secondary heat treatment, the metal temperature is rapidly raised to 420-450°C at a rate of 50-55°C / h, kept warm for 4-6 hours, the furnace gas temperature is reduced to 300°C at a rate of 30°C / h, and immediately taken out of the furnace for cooling.

[0014] (6) Finishing rolling: The material from step (5) is transferred to a foil rolling mill and rolled for 1-2 times to a finished product of 0.25-0.35 mm, wherein the rolling oil additive is controlled at 4-8% (weight percentage), the online plate shape is controlled at 3-5I, and the rolling oil temperature is controlled at 38-45°C. After the finished product is off the line, the second phase particle size and distribution are checked. The second phase particle distribution area accounts for ≤10%.

[0015] The finished raw material performance of this kind of low-density distributed second-phase particle aluminum foil material for new energy lithium-ion soft-pack batteries is 50-60Hv in Vickers hardness, 150-170Mpa in tensile strength, ≥3.0% in elongation, the second-phase particle size is controlled at 1-6μm, and the second-phase particle distribution area accounts for ≤10%.

[0016] Beneficial effects:

[0017] Compared with the aluminum foil material for new energy lithium-ion soft-pack batteries produced by traditional hot rolling + cold rolling, the production process of the aluminum foil material for new energy lithium-ion soft-pack batteries of the present invention has the advantages of short process and low energy consumption. The technical innovation has the following advantages:

[0018] (a) Fe and Si elements are added in the form of master alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before being added to the melting furnace. On the one hand, the addition of the master alloy eliminates the segregation of Fe and Si caused by the agglomeration of Fe agent and quick-dissolving silicon, which affects the subsequent processing of the billet;

[0019] (b) At the same time, the online three-stage filtration is used to eliminate aluminum liquid inclusions and mixed inert protective gas is introduced to prevent aluminum liquid from slagging;

[0020] (c) Using the "U"-shaped and "W"-shaped composite refining technology of the melting furnace, the aluminum melt is fully refined to ensure the purity of the aluminum melt. After the refining is completed, an inert protective gas is introduced into the furnace to prevent the aluminum liquid from oxidation;

[0021] (d) The homogenization process and the cold and foil rolling processes are optimized, so that the particles of the material tend to be dispersed, the particle size is small and uniform, the second phase particle size is controlled to be 1-6μm, and the distribution area of ​​the second phase particles accounts for ≤10%;

[0022] (e) At the same time, Cu element is appropriately added to form Al2Cu phase. On the one hand, the particle phase is solid-dissolved in the aluminum matrix to form solid solution strengthening, which improves the strength and Vickers hardness of the material. On the other hand, Al2Cu phase serves as the nucleation core of new recrystallized grains, which is beneficial to refine the matrix structure, thereby improving the comprehensive performance of the material.

[0023] As a result, the finished raw material performance of the aluminum foil material for new energy lithium-ion soft-pack batteries of the present invention has a Vickers hardness of 50-60Hv, a tensile strength of 150-170Mpa, an elongation of ≥3.0%, a second phase particle size controlled at 1-6μm, and a second phase particle distribution area ratio of ≤10%.

[0024] Compared with the second phase particle density of 50%-80% of the finished raw material of aluminum foil material for lithium-ion soft-pack batteries produced by the prior art, the product of the present invention has a low-density distributed second phase particles, and the second phase particle distribution area accounts for ≤10%, which is far better than the existing level and is conducive to deep drawing in subsequent processing. The product has a wide application market. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a distribution diagram of the second phase particles of the finished product in Example 1;

[0026] Figure 2 is a distribution diagram of the second phase particles of the finished product in Example 2;

[0027] Figure 3 This is a diagram showing the distribution of the second phase particles in the finished product of Comparative Example 1;

[0028] Figure 4 This is a diagram showing the distribution of the second phase particles in the finished product of Comparative Example 2. DETAILED DESCRIPTION

[0029] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0030] Embodiment 1:

[0031] (1) Preparation of alloy composition: The alloy elements are proportioned according to the following formula: Fe content is 1.4%, Si content is 0.03%, Ti content is 0.01%, Cu element is 0.002%, and the balance is aluminum, wherein the sum of the weight percentages of Fe, Si, Cu, Ti and Al is 100%.

[0032] (2) Melting: Fe and Si elements are added in the form of intermediate alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before adding to the melting furnace. After 1 / 3 of the aluminum liquid is flattened, Si and Fe elements are added to the melting furnace, and a covering agent of 3kg / t aluminum liquid is added simultaneously to prevent the aluminum liquid from further oxidation and slag formation. The refining process is carried out for 4 hours, and the refining agent is added at a ratio of 0.8kg / t aluminum liquid. At the same time, argon gas is introduced for powder blowing refining, and the refining is controlled for 30 minutes; after the "return" and "W" type operations are completed, argon gas is introduced into the melting furnace to maintain positive pressure in the furnace and keep it still for 1 hour. When no slag is visible on the surface of the aluminum liquid, the furnace pouring process is carried out.

[0033] (3) Online multi-stage composite filtration technology: The aluminum liquid treated in step (2) is passed into a filter box, which adopts a combination of tubular and plate filtration processes. The first-stage filter plate has a mesh number of 50 Ppi, the temperature in the insulation box is controlled at 725°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 1:1) is passed into the filter box; the second-stage filter plate has a mesh number of 70 Ppi, the temperature in the insulation box is controlled at 720°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 2:1) is passed into the filter box; the third-stage filter plate is a tubular filter RC grade, with a mesh number of 100 Ppi, the temperature in the insulation box is controlled at 710°C, and argon is passed into the filter box; then the aluminum liquid passes through a casting and rolling mill to obtain a cast-rolled coil billet with a thickness of 8.0 mm. The casting and rolling zone has a length of 45 mm, an opening of 13 mm, and a liquid level fluctuation control of 2 mm.

[0034] (4) Heat treatment technology: The cast-rolled coil obtained in step (3) is rolled for one pass and then heat treated. The outer ring is welded, the steel strip is tightened on the plate surface, and homogenization annealing is carried out in a high-temperature annealing furnace, and the furnace gas temperature is kept at 240°C for 10 hours. Then the temperature is raised to the target heating temperature of 500°C at 1°C / min, and the temperature is kept for 5 hours after reaching the target heating temperature. Then the furnace gas temperature is cooled at 3°C / min. When the furnace gas temperature reaches 350°C, it is immediately taken out of the furnace and air-cooled to obtain a semi-finished aluminum coil.

[0035] (5) Cold rolling and secondary heat treatment: The semi-finished product obtained in step (4) is rolled to 0.50 mm, wherein the crown of the cold rolling mill support roll is controlled at 0.03 mm, the roughness Ra value is 0.5 μm, the online plate shape is controlled at 10I during rolling, the oil temperature is controlled at 33°C, the oil nozzle flow rate is controlled at 40%, and the oil acid value is controlled at 0.3 mgKOH / g. The semi-finished product 0.5 mm is transferred to the annealing furnace for secondary heat treatment, the metal temperature is rapidly raised to 420°C at a rate of 50°C / h, kept warm for 4 hours, the furnace gas temperature is reduced to 300°C at a rate of 30°C / h, and immediately taken out of the furnace for cooling.

[0036] (6) Finishing rolling: The material from step (5) is transferred to the foil rolling mill and rolled to a finished product of 0.25 mm after 1-2 rolling steps, wherein the rolling oil additive is controlled at 4% (weight percentage), the online plate shape is controlled at 3I, and the rolling oil temperature is controlled at 38°C. After the finished product is off the line, the second phase particle size and distribution are checked, see Figure 1 shown.

[0037] The present invention obtains a finished raw material of an aluminum foil material for new energy lithium-ion soft-pack batteries with low-density distributed second-phase particles, the Vickers hardness of which is 50Hv, the tensile strength is 150Mpa, the elongation is 3.3%, the average size of the second-phase particles is controlled to be 3μm, and the distribution area of ​​the second-phase particles accounts for 5.6%.

[0038] Embodiment 2:

[0039] (1) Preparation of alloy composition: The alloy elements are proportioned according to the following formula: Fe content is 1.5%, Si content is 0.05%, Ti content is 0.02%, Cu element is 0.0035%, and the balance is aluminum, wherein the sum of the weight percentages of Fe, Si, Cu, Ti and Al is 100%.

[0040] (2) Melting: Fe and Si elements are added in the form of intermediate alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before adding to the melting furnace. After 1 / 3 of the aluminum liquid is flattened, Si and Fe elements are added to the melting furnace, and a covering agent of 4kg / t aluminum liquid is added simultaneously to prevent the aluminum liquid from further oxidation and slag formation. The refining process is carried out for 5 hours, and the refining agent is added at a ratio of 1.2kg / t aluminum liquid. At the same time, argon gas is introduced for powder blowing refining, and the refining is controlled for 30 minutes; after the "return" and "W" type operations are completed, argon gas is introduced into the melting furnace to maintain positive pressure in the furnace and keep it still for 1 hour. When no slag is visible on the surface of the aluminum liquid, the furnace pouring process is carried out.

[0041] (3) Online multi-stage composite filtration technology: The aluminum liquid treated in step (2) is passed into the filter box, which adopts a combination of tubular and plate filtration technology. The first-stage filter plate has a mesh number of 50 Ppi, the temperature in the insulation box is controlled at 730°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 1:1) is passed into the filter box; the second-stage filter plate has a mesh number of 70 Ppi, the temperature in the insulation box is controlled at 725°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 2:1) is passed into the filter box; the third-stage filter plate is a tubular filter RC grade, the mesh number is 100 Ppi, the temperature in the insulation box is controlled at 715°C, and argon is passed into the filter box; then the aluminum liquid passes through the casting and rolling mill to obtain a cast-rolled coil billet with a thickness of 8.5 mm. The casting and rolling zone has a length of 52 mm, an opening of 13 mm, and a liquid level of 4 mm for fluctuation control.

[0042] (4) Heat treatment technology: The cast-rolled coil obtained in step (3) is rolled for one pass and then heat treated. The outer ring is welded, the steel strip is tightened on the plate surface, and homogenization annealing is carried out in a high-temperature annealing furnace, and the furnace gas temperature is kept at 240°C for 10 hours. Then the temperature is increased at 1.5°C / min to the target heating temperature of 560°C, and the temperature is kept for 8 hours after reaching the target heating temperature. Then the furnace gas temperature is cooled at 4°C / min. When the furnace gas temperature reaches 350°C, it is immediately taken out of the furnace and air-cooled to obtain a semi-finished aluminum coil.

[0043] (5) Cold rolling and secondary heat treatment: The semi-finished product obtained in step (4) is rolled to 1.0 mm, wherein the crown of the cold rolling mill support roll is controlled at 0.03 mm, the roughness Ra value is 0.7 μm, the line plate shape is controlled at 12I during rolling, the oil temperature is controlled at 37°C, the oil nozzle flow rate is controlled at 45%, and the oil acid value is controlled at 0.4 mgKOH / g. The semi-finished product 1.0 mm is transferred to the annealing furnace for secondary heat treatment, the metal temperature is rapidly raised to 450°C at a rate of 55°C / h, kept at this temperature for 6 hours, the furnace gas temperature is reduced to 300°C at a rate of 30°C / h, and immediately taken out of the furnace for cooling.

[0044] (6) Finishing rolling: The material from step (5) is transferred to the foil rolling mill and rolled to a finished product of 0.35 mm after 2 rollings, wherein the rolling oil additive is controlled at 8% (weight percentage), the online plate shape is controlled at 5I, and the rolling oil temperature is controlled at 45°C. After the finished product is off the line, the second phase particle size and distribution are checked, see Figure 2 shown.

[0045] The present invention obtains an aluminum foil material for new energy lithium-ion soft-pack batteries with low-density distributed second-phase particles. The finished raw material performance is 60Hv in Vickers hardness, 170Mpa in tensile strength, 3.0% in elongation, the average size of the second-phase particles is controlled to be 5μm, and the distribution area of ​​the second-phase particles accounts for 7.8%.

[0046] Comparative Example 1:

[0047] (1) Preparation of alloy composition: The alloy elements are proportioned according to the following formula: Fe content is 1.4%, Si content is 0.03%, Ti content is 0.01%, Cu element is 0.002%, and the balance is aluminum, wherein the sum of the weight percentages of Fe, Si, Cu, Ti and Al is 100%.

[0048] (2) Melting: Fe and Si elements are added in the form of intermediate alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before adding to the melting furnace. After 1 / 3 of the aluminum liquid is flattened, Si and Fe elements are added to the melting furnace, and a covering agent of 3kg / t aluminum liquid is added simultaneously to prevent the aluminum liquid from further oxidation and slag formation. The refining process is carried out for 4 hours, and the refining agent is added at a ratio of 0.8kg / t aluminum liquid. At the same time, argon gas is introduced for powder blowing refining, and the refining is controlled for 30 minutes; after the "return" and "W" type operations are completed, argon gas is introduced into the melting furnace to maintain positive pressure in the furnace and keep it still for 1 hour. When no slag is visible on the surface of the aluminum liquid, the furnace pouring process is carried out.

[0049] (3) Online multi-stage composite filtration technology: The aluminum liquid treated in step (2) is passed into a filter box, which adopts a combination of tubular and plate filtration processes. The first-stage filter plate has a mesh number of 50 Ppi, the temperature in the insulation box is controlled at 725°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 1:1) is passed into the filter box; the second-stage filter plate has a mesh number of 70 Ppi, the temperature in the insulation box is controlled at 720°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 2:1) is passed into the filter box; the third-stage filter plate is a tubular filter RC grade, with a mesh number of 100 Ppi, the temperature in the insulation box is controlled at 710°C, and argon is passed into the filter box; then the aluminum liquid passes through a casting and rolling mill to obtain a cast-rolled coil billet with a thickness of 8.0 mm. The casting and rolling zone has a length of 45 mm, an opening of 13 mm, and a liquid level fluctuation control of 2 mm.

[0050] (4) Heat treatment technology: The cast-rolled coil obtained in step (3) is heat treated after rolling for one pass at a furnace temperature of 500°C for 20 hours, and then air-cooled immediately after being taken out of the furnace to obtain a semi-finished aluminum coil.

[0051] (5) Cold rolling and secondary heat treatment: The semi-finished product obtained in step (4) is rolled to 0.50 mm, wherein the crown of the cold rolling mill support roll is controlled at 0.03 mm, the roughness Ra value is 0.5 μm, the online plate shape is controlled at 10I during rolling, the oil temperature is controlled at 33°C, the oil nozzle flow rate is controlled at 40%, and the oil acid value is controlled at 0.3 mgKOH / g. The semi-finished product 0.5 mm is transferred to the annealing furnace for secondary heat treatment, the metal temperature is rapidly raised to 420°C at a rate of 50°C / h, kept warm for 6 hours, the furnace gas temperature is reduced to 300°C at a rate of 30°C / h, and immediately taken out of the furnace for cooling.

[0052] (6) Finishing rolling: The material from step (5) is transferred to the foil rolling mill and rolled to a finished product of 0.25 mm after 1-2 rolling steps, wherein the rolling oil additive is controlled at 4% (weight percentage), the online plate shape is controlled at 3I, and the rolling oil temperature is controlled at 38°C. After the finished product is off the line, the second phase particle size and distribution are checked, see Figure 3 shown.

[0053] The finished product rough material performance of this kind of aluminum foil material is Vickers hardness 50Hv, tensile strength 150Mpa, elongation 3.3%, and the second phase particle distribution area accounts for 65%. This kind of product cannot meet the requirements.

[0054] Comparative Example 2:

[0055] (1) Preparation of alloy composition: The alloy elements are proportioned according to the following formula: Fe content is 1.7%, Si content is 0.05%, Ti content is 0.02%, Cu element is 0.05%, and the balance is aluminum, wherein the sum of the weight percentages of Fe, Si, Cu, Ti and Al is 100%.

[0056] (2) Melting: Fe and Si elements are added in the form of intermediate alloys, with a ratio of Al-20% Fe and Al-20% Si. The surface oxide film is removed by a milling machine before adding to the melting furnace. After 1 / 3 of the aluminum liquid is flattened, Si and Fe elements are added to the melting furnace, and a covering agent of 4kg / t aluminum liquid is added simultaneously to prevent the aluminum liquid from further oxidation and slag formation. The refining process is carried out for 5 hours, and the refining agent is added at a ratio of 1.2kg / t aluminum liquid. At the same time, argon gas is introduced for powder blowing refining, and the refining is controlled for 30 minutes; after the "return" and "W" type operations are completed, argon gas is introduced into the melting furnace to maintain positive pressure in the furnace and keep it still for 1 hour. When no slag is visible on the surface of the aluminum liquid, the furnace pouring process is carried out.

[0057] (3) Online multi-stage composite filtration technology: The aluminum liquid treated in step (2) is passed into a filter box, which adopts a combination of tubular and plate filtration technology. The first-stage filter plate mesh number is 50 PPi, the temperature in the insulation box is controlled at 730°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 1:1) is passed into the filter box; the second-stage filter plate mesh number is 70 PPi, the temperature in the insulation box is controlled at 725°C, and a nitrogen and argon mixed gas (volume ratio, argon: nitrogen = 2:1) is passed into the filter box; then the aluminum liquid passes through a casting and rolling mill to obtain a cast-rolled coil billet with a thickness of 8.5 mm. The casting and rolling zone length is 52 mm, the opening is 13 mm, and the liquid level is controlled by fluctuation of 4 mm.

[0058] (4) Heat treatment technology: The cast-rolled coil obtained in step (3) is rolled for one pass and then heat treated. The outer ring is welded, the steel strip is tightened on the plate surface, and homogenization annealing is carried out in a high-temperature annealing furnace at a furnace gas temperature of 240°C for 10 hours. Then, the furnace gas temperature is 560°C, and after reaching the target heating temperature, it is kept warm for 8 hours. After that, the furnace gas temperature is cooled at 4°C / min. When the furnace gas temperature reaches 350°C, it is immediately taken out of the furnace and air-cooled to obtain a semi-finished aluminum coil.

[0059] (5) Cold rolling and secondary heat treatment: The semi-finished product obtained in step (4) is rolled to 1.0 mm, wherein the crown of the cold rolling mill support roll is controlled at 0.03 mm, the roughness Ra value is 0.7 μm, the line plate shape is controlled at 12I during rolling, the oil temperature is controlled at 37°C, the oil nozzle flow rate is controlled at 45%, and the oil acid value is controlled at 0.4 mgKOH / g. The semi-finished product 1.0 mm is transferred to the annealing furnace for secondary heat treatment, the metal temperature is 450°C, and it is kept warm for 5 hours before being taken out of the furnace for cooling.

[0060] (6) Finishing rolling: The material from step (5) is transferred to the foil rolling mill and rolled to a finished product of 0.35 mm after 2 rollings, wherein the rolling oil additive is controlled at 8% (weight percentage), the online plate shape is controlled at 5I, and the rolling oil temperature is controlled at 45°C. After the finished product is off the line, the second phase particle size and distribution are checked, see Figure 4 shown.

[0061] The finished product raw material performance of this kind of aluminum foil material is Vickers hardness 60Hv, tensile strength 170Mpa, elongation ≥3.0%, the average size of the second phase particles is controlled at 5μm, and the distribution area of ​​the second phase particles accounts for 75%. This product cannot meet the requirements.

[0062] It can be seen that in Example 1-2, by optimizing the homogenization treatment process and the cold and foil rolling process, the particles of the material tend to be dispersed, the particle size is small and uniform, the second phase particle size is controlled to be 1-6μm, and the distribution area of ​​the second phase particles accounts for ≤10%; thereby meeting the use requirements. In Comparative Example 1-2, although the mechanical properties are similar, the distribution of the second phase particles is too large to meet the subsequent production and preparation requirements of aluminum foil materials for batteries.

[0063] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a battery aluminum foil material with low-density distributed second phase particles, characterized in that: The alloy composition includes 1.4-1.5% Fe, 0.03-0.05% Si, 0.01-0.02% Ti, 0.002-0.0035% Cu in terms of mass percentage, and the rest is aluminum and unavoidable impurities; The preparation process comprises the following steps: S1. Smelting: After the aluminum is 1 / 3 flattened, Fe and Si in the form of a master alloy are added to the smelting furnace, and an anti-oxidation covering agent is added simultaneously; S2. Refining: During the refining process, a refining agent is added at a ratio of 0.8-1.2 kg / t aluminum liquid, and argon gas is introduced at the same time for powder blowing refining; S3, furnace pouring and forming: the molten aluminum water is passed into the filter box, and after several filtrations, it is passed through the casting and rolling mill to prepare the cast and rolled coil blank; S4, first heat treatment: homogenizing annealing of the cast-rolled coil blank; S5, cold rolling: cold rolling the billet after the first heat treatment to prepare a semi-finished billet of 0.5-1.0 mm; S6. Second heat treatment: The semi-finished blank is subjected to a second heat treatment, wherein the metal temperature is rapidly raised to 420-450°C at a rate of 50-55°C / h, kept at this temperature for 4-6 hours, and then the furnace gas temperature is controlled to drop to 300°C at a rate of 30°C / h, and the blank is immediately taken out of the furnace for cooling; S7, transferring the cooled billet to a foil rolling mill, and rolling the billet for 1-2 times to a finished product of 0.25-0.35 mm, wherein the rolling oil additive is controlled at 4-8% by weight, the online plate shape is controlled at 3-5I, and the rolling oil temperature is controlled at 38-45°C; after the finished product is off the line, the second phase particle size and distribution are inspected; When Fe and Si are added for smelting, the ratio of the master alloy is Al-20%Fe and Al-20%Si, wherein the oxide film on the surface of the master alloy is removed before smelting; During the refining process, exhaust is carried out through "return" or "W" type operation, and the refining furnace is kept in a positive pressure state. After standing for 0.8 to 2 hours, when no slag can be detected by visual method, the furnace pouring process is carried out; The aluminum liquid is filtered by combining tubular and plate filtration, wherein the mesh number of the first-stage filter plate is 50PPi, and the insulation temperature during the first-stage filtration is 725-730°C; the mesh number of the second-stage filter plate is 70PPi, and the insulation temperature during the second-stage filtration is 720-725°C; the third-stage filtration is tubular filtration, the mesh number is 100PPi, and the insulation temperature during the third-stage filtration is 710-715°C. After the filtration is completed, it is prepared into a cast-rolled coil billet with a thickness of 8.0-8.5mm through a casting and rolling mill; In the first heat treatment, the furnace gas temperature is 240℃, kept warm for 10 hours, then heated to the target heating temperature of 500-560℃ at a rate of 1-1.5℃ / min, and kept warm for 5-8 hours after reaching the target heating temperature. Then the furnace gas temperature is cooled at a rate of 3-4℃ / min. When the furnace gas temperature reaches 350℃, it is immediately taken out of the furnace and air-cooled to obtain a semi-finished aluminum coil.

2. The method for preparing a battery aluminum foil material with low-density distributed second phase particles according to claim 1, characterized in that: During the first stage of filtration, argon and nitrogen in a volume ratio of 1:1 were passed through, during the second stage of filtration, argon and nitrogen in a volume ratio of 2:1 were passed through, and during the third stage of filtration, argon was passed through.

3. The method for preparing a battery aluminum foil material with low-density distributed second phase particles according to claim 1, characterized in that: During the casting and rolling process, the casting and rolling zone has a length of 45-52 mm, an opening of 13 mm, and a liquid level fluctuation control of 2-4 mm.

4. The method for preparing a battery aluminum foil material with low-density distributed second phase particles according to claim 1, characterized in that: During cold rolling, the crown of the cold rolling mill support roll is controlled at 0.03mm, the roughness Ra value is 0.5-0.7μm, the online plate shape is controlled at 10-12I during rolling, the oil temperature is controlled at 33-37℃, the oil nozzle flow is controlled at 40-45%, and the oil acid value is controlled at 0.3-0.4mgKOH / g.

5. The method for preparing a battery aluminum foil material with low-density distributed second phase particles according to claim 1, characterized in that: When the finished product is inspected off-line, the distribution area of ​​the second phase particles shall account for ≤10%.