A Cu2O / COFs core-shell cubic photocatalyst and its preparation method and application
Through the preparation of Cu2O/COFs core-shell cube photocatalyst, the COFs shell is formed by using Schiff alkali reaction to cover Cu2O cubes, which solves the problems of low activity and easy corrosion of metal oxide photocatalysts, and achieves efficient photocatalytic hydrogen production and Resistant photocorrosion.
Patent Information
- Application Number
- CN202310005979.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-01-04
AI Technical Summary
Metal oxide photocatalysts have low catalytic activity and are prone to photocorrosion in the photocatalytic hydrogen production process, and it is difficult to effectively improve their stability.
The preparation method of Cu2O/COFs core-shell cube photocatalyst is adopted. By reacting Cu2O cube with amino and aldehyde organic ligands, the COFs shell cover is formed, which improves photocatalytic activity and inhibits photocorrosion.
The high photocatalytic activity and excellent photocorrosion resistance of Cu2O/COFs core-shell cube photocatalysts are achieved, which significantly improves the stability of the catalyst and hydrogen production rate.
Smart Images

Figure HDA0004036730610000011 
Figure HDA0004036730610000012 
Figure HDA0004036730610000013
Abstract
Description
Technical Field
[0001] The invention relates to the field of photocatalysis, and in particular to a Cu2O / COFs core-shell cubic photocatalyst and a preparation method and application thereof. Background Art
[0002] The continuous consumption of fossil energy has led to severe energy crises and environmental problems. Hydrogen is considered an ideal energy source to replace fossil energy because of its high energy density (142MJ / kg) and its lack of geographical and temporal restrictions. Photocatalytic hydrogen production technology directly converts sustainable solar energy into clean hydrogen energy, which is a rational way to solve the energy crisis and environmental problems. The development of new high-performance photocatalysts is an important prerequisite for the practical application of photocatalytic hydrogen production.
[0003] Metal oxides are widely used in photocatalytic hydrogen production research due to their advantages such as low price, adjustable band gap, excellent light absorption performance and photogenerated carrier properties. However, the serious photogenerated carrier recombination of metal oxides (such as Cu2O) themselves leads to poor photocatalytic activity. In addition, the photocorrosion of the catalyst during the catalytic process will also lead to a decrease in its stability. Although many metal oxide heterojunction semiconductor materials have been developed to significantly improve the catalytic activity of metal oxides, the problem of catalyst photocorrosion is difficult to effectively solve.
[0004] Two-dimensional covalent organic framework materials (COFs) are ordered porous crystals connected by covalent bonds. In recent years, they have been widely studied and applied in the fields of photocatalysis, electrocatalysis, gas separation, and electronic devices. Among them, COFs materials represented by Schiff bases have advantages such as broad light absorption performance, high conjugation, corrosion resistance, adjustable structure, and controllable band gap, showing application potential in the field of photocatalysis. Therefore, constructing a heterojunction of metal oxides and COFs will not only promote the separation of photogenerated carriers, but also effectively inhibit the photocorrosion of the catalyst, which is of great significance for the development of new high-performance photocatalysts. Summary of the invention
[0005] Based on the shortcomings of low catalytic activity and easy photocorrosion faced by the current Cu2O photocatalytic hydrogen production, the present invention provides a Cu2O / COFs core-shell cubic photocatalyst and a preparation method and application thereof. The Cu2O / COFs core-shell cubic photocatalyst has high photocatalytic activity and excellent anti-photocorrosion performance.
[0006] The present invention first provides a method for preparing a Cu2O / COFs core-shell cubic photocatalyst, comprising the following steps:
[0007] The Cu2O cube is mixed with an amino organic ligand, and the amino organic ligand is anchored on the surface of the Cu2O cube by utilizing the interaction force between the amino group and copper; then, an aldehyde organic ligand and a catalyst are added to react, so that the amino organic ligand and the aldehyde organic ligand undergo a Schiff base reaction on the surface of the Cu2O cube, thereby obtaining the Cu2O / COFs core-shell cube photocatalyst.
[0008] The above-mentioned preparation method specifically comprises the following steps:
[0009] 1) Dispersing Cu2O cubes and amino organic ligands into a mixed solution of n-butanol and o-dichlorobenzene;
[0010] 2) The solution of step 1) is mixed with an aldehyde organic ligand and a catalyst to perform a Schiff base reaction to obtain the Cu2O / COFs core-shell cubic photocatalyst.
[0011] In the above preparation method, the amino organic ligand is at least one of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene, 5,10,15,20-tetrakis(4-aminophenyl)-21H,23H-porphyrin, 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine;
[0012] The aldehyde-based organic ligand is at least one of terephthalaldehyde, 2,5-dihydroxyterephthalaldehyde, 2,3,5,6-tetrafluorobenzaldehyde and 2,5-dimethoxybenzene-1,4-dicarboxaldehyde; specifically, it can be terephthalaldehyde;
[0013] The catalyst is at least one of p-toluenesulfonic acid and acetic acid; specifically, it can be p-toluenesulfonic acid;
[0014] The mass ratio of the amino organic ligand to the Cu2O cube is 0.1-1:1; specifically, it can be 0.1-0.5:1; more specifically, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1 or 0.48:1.
[0015] The mass ratio of the aldehyde organic ligand to the amino organic ligand is 0.5 to 3:2; specifically, it can be 1:2 or 0.8:2;
[0016] The mass ratio of the catalyst to the amino organic ligand is 0.04 to 2:1; specifically, it can be 0.1:1, 0.07:1, 0.05:1 or 0.04:1.
[0017] In the above preparation method, the temperature of the Schiff base reaction is 50°C to 150°C, preferably 100°C to 120°C.
[0018] In the above preparation method, the reaction time of the Schiff base is 0.5h-100h; preferably 24h-100h;
[0019] The Schiff base reaction is carried out in a vacuum sealed tube.
[0020] In the above preparation method, the volume ratio of n-butanol to o-dichlorobenzene in the mixed solution of n-butanol and o-dichlorobenzene is 0.5 to 2:1, and can be specifically 1:1.
[0021] The above-mentioned preparation method, step 1) further comprises the steps of dispersing Cu2O cubes and amino organic ligands into a mixed solution of n-butanol and o-dichlorobenzene and then performing ultrasonic treatment and stirring in sequence;
[0022] Specifically, the ultrasonic time is 10 min to 50 min, and the ultrasonic frequency is 50 Hz to 100 Hz;
[0023] Specifically, the stirring time is 10 min to 100 min, and the stirring speed is 50 rpm to 300 rpm;
[0024] The purpose of the above-mentioned ultrasound and stirring is to disperse the sample evenly, and the specific conditions have little effect on the structure of the obtained product and the catalytic effect.
[0025] In step 2), after the Schiff base reaction, there are steps of centrifuging to obtain a sample, washing the sample and drying the sample;
[0026] Specifically, the sample is washed with tetrahydrofuran; the number of washing times is 3 to 5 times;
[0027] Specifically, the drying condition is drying at 90° C. for 2 h to 10 h.
[0028] In the above-mentioned preparation method, the specific operation of step 2) includes adding an aldehyde organic ligand to the solution of step 1), ultrasonicating, and then adding a catalyst to carry out a Schiff base reaction to obtain the Cu2O / COFs core-shell cubic photocatalyst;
[0029] Specifically, the ultrasonic time is 10 min to 50 min, and the ultrasonic frequency is 50 Hz to 100 Hz.
[0030] The ultrasound in step 2) is also to make the sample dispersed evenly, and the frequency and time of the ultrasound have little effect on the structure and catalytic effect of the photocatalyst.
[0031] In the above-mentioned preparation method, the preparation method of the Cu2O cube is a conventional method known to those skilled in the art, and specifically comprises the following steps: mixing CuSO4·5H2O, sodium citrate and water, then adding NaOH solution and L-ascorbic acid solution, stirring and aging to obtain the Cu2O cube.
[0032] The present invention also provides a Cu2O / COFs core-shell cubic photocatalyst prepared by the above preparation method.
[0033] The COFs shell thickness of the Cu2O / COFs core-shell cubic photocatalyst is 8 to 30 nm, and can be specifically 9.8 nm, 16.6 nm, 20.2 nm, 24.7 nm or 29.6 nm.
[0034] The application of the above-mentioned Cu2O / COFs core-shell cubic photocatalyst in the photocatalytic hydrogen production reaction also falls within the protection scope of the present invention.
[0035] The Cu2O / COFs core-shell cubic photocatalyst prepared by the present invention can show 12.5 mmol h -1 g -1 hydrogen production rate.
[0036] Compared with the prior art, the present invention has the following advantages:
[0037] The Cu2O / COFs core-shell cubic photocatalyst prepared by the pre-deposition method of the present invention has a simple preparation process and has the advantages of controllable shell thickness, high photocatalytic activity and resistance to light corrosion. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a transmission electron microscopy image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 1.
[0039] Figure 2 This is a transmission electron micrograph of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 2.
[0040] Figure 3 This is a transmission electron microscope image of Cu2O cubes after being used for photocatalytic hydrogen production.
[0041] Figure 4 This is a scanning electron microscope image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 2 after photocatalysis.
[0042] Figure 5 This is a transmission electron micrograph of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 3.
[0043] Figure 6This is a transmission electron micrograph of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 4.
[0044] Figure 7 This is a transmission electron micrograph of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 5.
[0045] Figure 8 It is a photocatalytic hydrogen production performance diagram of the photocatalysts of Examples 1 to 5.
[0046] Fig. 9 It is a comparison chart of the photocatalytic hydrogen production performance of the photocatalysts of Example 4 and Example 6.
[0047] Fig.10 It is a comparison chart of the photocatalytic hydrogen production performance of the photocatalysts of Example 4 and Comparative Example 1. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0049] The experimental methods in the following examples are all conventional methods unless otherwise specified.
[0050] The quantitative tests in the following examples were all repeated three times, and the results were averaged.
[0051] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0052] The Cu2O cubes in the following examples were prepared by our laboratory, and the specific steps are as follows: 375 mg CuSO4·5H2O and 147 mg sodium citrate were added to 80 mL deionized water and stirred at 100 rpm for 20 min. Then, 20 mL of 1.25 M NaOH solution was added and stirred at 100 rpm for 15 min. Subsequently, 50 mL of 0.03 M L-ascorbic acid was added and the solution was stirred for 15 min. Then, it was aged for 1 h. Finally, the Cu2O cubes were obtained by centrifugation, deionized water washing, ethanol washing and drying.
[0053] Example 1
[0054] 1) Weigh 50 mg Cu2O cubes and 5 mg 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 50 Hz for 10 min, and stir at 100 rpm for 1 h.
[0055] 2) Weigh 2.5 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasonication at 50 Hz for 20 min; then add 0.5 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 120° C. for 72 h.
[0056] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 10 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0057] The Cu2O / COFs core / shell cubic photocatalyst prepared as above was used for photocatalytic hydrogen production test.
[0058] Figure 1 is a transmission electron microscopy image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 1, Figure 1 It can be seen that the photocatalyst prepared by the method of the present invention has a structure in which COFs encapsulate Cu2O cubic blocks, wherein the COFs shell thickness is about 9.8 nm.
[0059] Example 2
[0060] 1) Weigh 50 mg Cu2O cubes and 10 mg 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 80 Hz for 20 min, and stir at 150 rpm for 1.5 h.
[0061] 2) Weigh 5 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasonication at 50 Hz for 20 min; then add 1 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 120° C. for 72 h.
[0062] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 8 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0063] The Cu2O / COFs core / shell cubic photocatalyst prepared as above was used for photocatalytic hydrogen production test.
[0064] Figure 2 is a transmission electron micrograph of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 2. Figure 2 It can be seen that the COFs shell thickness is about 16.6 nm.
[0065] Figure 3 This is a transmission electron microscope image of a pure Cu2O cube after being used for photocatalytic hydrogen production. Figure 3 It can be seen that the pure Cu2O cubes underwent obvious photocorrosion after 20 hours of photocatalysis, and the catalyst was destroyed. Figure 4 This is a SEM image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 2 after 50 hours of photocatalysis, and the catalyst still has excellent morphology. It can be seen that the Cu2O / COFs core / shell cubic photocatalyst can significantly improve the corrosion resistance of the photocatalyst.
[0066] Example 3
[0067] 1) Weigh 50 mg Cu2O cubes and 15 mg 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 50 Hz for 30 min, and stir at 200 rpm for 1.5 h.
[0068] 2) Weigh 7.5 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasonication at 50 Hz for 10 min; then add 1 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 120° C. for 72 h.
[0069] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 8 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0070] The Cu2O / COFs core / shell cubic photocatalyst prepared as above was used for photocatalytic hydrogen production test.
[0071] Figure 5 is a transmission electron microscopy image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 3. Figure 5 It can be seen that the COFs shell thickness is about 20.2 nm.
[0072] Example 4
[0073] 1) Weigh 50 mg Cu2O cubes and 20 mg 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 50 Hz for 30 min, and stir at 100 rpm for 1.5 h.
[0074] 2) Weigh 10 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasound at 50 Hz for 10 min; then add 1 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 115° C. for 72 h.
[0075] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 8 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0076] The Cu2O / COFs core / shell cubic photocatalyst prepared as above was used for photocatalytic hydrogen production test.
[0077] Figure 6 is a transmission electron microscopy image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 4. Figure 6 It can be seen that the COFs shell thickness is about 24.7nm.
[0078] Example 5
[0079] 1) Weigh 50 mg Cu2O cubes and 25 mg 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 50 Hz for 30 min, and stir at 100 rpm for 1.5 h.
[0080] 2) Weigh 12.5 mg of terephthalaldehyde and add it to the reaction solution in step 1), and ultrasonicate at 50 Hz for 10 min; then add 1 mg of toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 100° C. for 72 h.
[0081] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 8 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0082] The Cu2O / COFs core / shell cubic photocatalyst prepared as above was used for photocatalytic hydrogen production test.
[0083] Figure 7 is a transmission electron microscopy image of the Cu2O / COFs core / shell cubic photocatalyst prepared in Example 5. Figure 7 It can be seen that the COFs shell thickness is 29.6nm.
[0084] The method for testing the photocatalytic hydrogen production of the Cu2O / COFs core / shell cubic photocatalyst in the above embodiment is as follows:
[0085] The photocatalytic reaction was carried out in a quartz reactor. 10 mg of the photocatalyst was added to a 10% (v:v) methanol aqueous solution and argon was introduced for 30 min. A 300W xenon lamp was used as the light source for the photocatalytic reaction, and the light intensity was AM1.5. The photocatalytic hydrogen production was detected by gas chromatography.
[0086] Figure 8 The performance test of photocatalytic hydrogen production of the samples corresponding to Examples 1 to 5 is as follows. Figure 8It can be seen that with the increase of COFs shell thickness, the photocatalytic performance shows a trend of first increasing and then decreasing. When the COFs shell thickness is 24.7 nm, the best photocatalytic performance can be obtained, and its photocatalytic hydrogen production activity is 12.5 mmol h -1 g -1 .
[0087] Example 6
[0088] 1) Weigh 50 mg Cu2O cubes and 24 mg 5,10,15,20-tetrakis(4-aminophenyl)-21H,23H-porphyrin into a mixed solution of 1.5 mL o-dichlorobenzene and 1.5 mL n-butanol, ultrasonicate at 50 Hz for 30 min, and stir at 200 rpm for 1.5 h.
[0089] 2) Weigh 10 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasonication at 50 Hz for 10 min; then add 1 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 120° C. for 72 h.
[0090] 3) The sample after the reaction in step 2) was centrifuged and washed with tetrahydrofuran solvent for 3 times, and dried at 90° C. for 8 h to obtain a Cu2O / COFs core / shell cubic photocatalyst.
[0091] The Cu2O / COFs core / shell cubic photocatalyst prepared above was used for photocatalytic hydrogen production test (the test method and conditions were the same as those in the above example), and the results are shown in Fig. 9 .Depend on Fig. 9 It can be seen that the photocatalyst activity prepared in Example 6 can reach 6.7 12.5 mmol h -1 g -1 , but lower than the performance of the photocatalyst prepared in Example 4.
[0092] Comparative Example 1
[0093] 1) Add 20 mg of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene to a mixed solution of 1.5 mL of o-dichlorobenzene and 1.5 mL of n-butanol, ultrasonicate at 50 Hz for 30 min, and stir at 100 rpm for 1.5 h.
[0094] 2) Weigh 10 mg of terephthalaldehyde and add it to the reaction solution in step 1), and perform ultrasound at 50 Hz for 10 min; then add 1 mg of p-toluenesulfonic acid as a catalyst, seal the reactor under vacuum, and react at 115° C. for 72 h.
[0095] 3) The COFs prepared in step 2 were centrifuged, washed three times with tetrahydrofuran solvent, and dried at 90° C. for 8 h.
[0096] 4) The COFs obtained in step 3) were physically mixed with Cu2O at a mass ratio of 0.4:1 as a photocatalyst to carry out a photocatalytic reaction. The test method and conditions were the same as those in the above embodiment.
[0097] Fig.10 The photocatalytic effect of physical mixing is significantly lower than that of COFs-coated Cu2O catalyst, indicating that COFs tightly encapsulating Cu2O can promote the transmission of electrons and improve the photocatalytic performance.
Claims
1. A method for preparing a Cu2O / COFs core-shell cubic photocatalyst, comprising the following steps: The Cu2O cube is mixed with an amino organic ligand, and the amino organic ligand is anchored on the surface of the Cu2O cube by utilizing the interaction force between the amino group and copper; then, an aldehyde organic ligand and a catalyst are added to react, so that the amino organic ligand and the aldehyde organic ligand undergo a Schiff base reaction on the surface of the Cu2O cube, thereby obtaining the Cu2O / COFs core-shell cube photocatalyst; The amino organic ligand is at least one of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene, 5,10,15,20-tetrakis(4-aminophenyl)-21H,23H-porphyrin, 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine; The aldehyde-based organic ligand is at least one of terephthalaldehyde, 2,5-dihydroxyterephthalaldehyde, 2,3,5,6-tetrafluorobenzaldehyde and 2,5-dimethoxybenzene-1,4-dicarbaldehyde.
2. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: 1) Dispersing Cu2O cubes and amino organic ligands into a mixed solution of n-butanol and o-dichlorobenzene; 2) The solution of step 1) is mixed with an aldehyde organic ligand and a catalyst to perform a Schiff base reaction to obtain the Cu2O / COFs core-shell cubic photocatalyst.
3. The preparation method according to claim 1 or 2, characterized in that: The catalyst is at least one of p-toluenesulfonic acid and acetic acid; The mass ratio of the amino organic ligand to the Cu2O cube is 0.1-1:1; The mass ratio of the aldehyde organic ligand to the amino organic ligand is 0.5-3:2; The mass ratio of the catalyst to the amino organic ligand is 0.04-2:
1.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The temperature of the Schiff base reaction is 50°C to 150°C.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The Schiff base reaction time is 0.5 h-100 h; The Schiff base reaction is carried out in a vacuum sealed tube.
6. The preparation method according to any one of claims 2 to 5, characterized in that: The volume ratio of n-butanol to o-dichlorobenzene in the n-butanol and o-dichlorobenzene mixed solution is 0.5-2:
1.
7. The preparation method according to any one of claims 2 to 6, characterized in that: Step 1) also includes the steps of dispersing Cu2O cubes and amino organic ligands in a mixed solution of n-butanol and o-dichlorobenzene and then performing ultrasonic treatment and stirring in sequence; Specifically, the ultrasound time is 10 min to 50 min, and the ultrasound frequency is 50 Hz to 100 Hz; Specifically, the stirring time is 10 min to 100 min, and the stirring speed is 50 rpm to 300 rpm; In step 2), after the Schiff base reaction, there are steps of centrifuging to obtain a sample, washing the sample and drying the sample; Specifically, the sample is washed with tetrahydrofuran; the number of washing times is 3 to 5 times; Specifically, the drying condition is drying at 90° C. for 2 h to 10 h.
8. The preparation method according to any one of claims 2 to 7, characterized in that: The specific operation of step 2) includes adding an aldehyde organic ligand to the solution of step 1), ultrasonicating, and then adding a catalyst to carry out a Schiff base reaction to obtain the Cu2O / COFs core-shell cubic photocatalyst; Specifically, the ultrasound time is 10 min to 50 min, and the ultrasound frequency is 50 Hz to 100 Hz.
9. The Cu2O / COFs core-shell cubic photocatalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the Cu2O / COFs core-shell cubic photocatalyst according to claim 9 in a photocatalytic hydrogen production reaction.
Citation Information
Patent Citations
Core-shell structure metal organic framework based composite photocatalyst and preparation method thereof
CN108479855A
Nano CuO / COF composite arsenic removal material and preparation method thereof
CN111704196A
Application of cuprous oxide nano-catalyst in electrocatalytic reduction of nitrate nitrogen
CN114540841A
In-situ growth graphene two-dimensional covalent organic framework composite material and preparation method thereof
CN114854214A
Organic-inorganic semiconductor hybrid dual-photoelectrode unbiased photoelectrocatalysis full-decomposition water hydrogen production method
CN115074746A