A composite flame retardant based on vermiculite and preparation method thereof
By treating vermiculite through acidification intercalation and amino coupling, and inserting flame retardants into its layers, the deficiencies in flame retardant performance and smoke suppression effect of halogen-free flame retardants are solved, and the compatibility of polymers is improved. properties and thermal stability, achieving better flame retardant effects.
Patent Information
- Application Number
- CN202310032855.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-10
AI Technical Summary
Existing halogen-free flame retardants have deficiencies in flame retardant performance and smoke suppression effect, and traditional flame retardants have poor compatibility with polymers, low adhesion, and poor thermal stability.
Using acidification intercalation, particle size flotation, amino coupling and flame retardant intercalation, the vermiculite is treated with tetramethylammonium bromide and aminosilane coupling agent to form a structure with interlayer space, and the three Flame retardants such as sodium polyphosphate are intercalated into the vermiculite layers to synergistically provide flame retardancy.
It improves the flame retardant and smoke suppression effect of the flame retardant, enhances the compatibility and adhesion with the polymer, improves the thermal stability, and achieves better flame retardant performance.
Smart Images

Figure BDA0004047950500000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a vermiculite-based composite flame retardant and a preparation method thereof. Background Art
[0002] Flame retardant is a functional additive that can make flammable polymers flame retardant. Flame retardants can be divided into additive flame retardants and reactive flame retardants according to the method of use. In recent years, people's environmental awareness has become stronger and stronger, and the requirements for fire safety and flame retardant products have become higher and higher. Halogen-free, low-smoke, low-toxic environmentally friendly flame retardants have become the goal pursued by people. Among them, inorganic flame retardants show good environmental performance, but the flame retardant performance is not as good as organic flame retardants. However, some organic flame retardants contain halogens, and due to their small molecular weight in polymers such as plastics and resins, they will migrate and precipitate.
[0003] At present, the halogen-free flame retardants that are being studied more are mainly calcium carbonate, aluminum hydroxide, magnesium hydroxide, layered silicate materials, inorganic phosphorus, boron, expanded graphite and other inorganic flame retardant materials, as well as organic nitrogen and phosphorus flame retardants, etc. Although halogen-free flame retardants have advantages such as environmental protection and low smoke, a single flame retardant component also has disadvantages such as poor flame retardant effect and poor smoke suppression effect.
[0004] Vermiculite has a monomolecular hydration layer between layers. Each layer of vermiculite is composed of silicon-oxygen tetrahedrons, which are connected by interlayer hydrogen bonds. Water molecules also connect each layer of silicon-oxygen tetrahedrons by hydrogen bonds, which greatly increases the thixotropy of the system. The melting point of vermiculite is 1370-1400℃, and the thermal conductivity is extremely low at 0.046W / (M·K). When heated by fire, the interlayer expands 2-40 times, and has excellent flame retardant properties.
[0005] Patent CN104804440B discloses a method for preparing a silicone rubber / vermiculite composite material, which is to react expanded vermiculite with diisocyanate to obtain isocyanate-modified expanded vermiculite, and form a layer of isocyanate active molecular film on the surface of the expanded vermiculite; then polymerize with condensed silicone rubber to form silicone rubber / expanded vermiculite prepolymer; finally, add silane coupling agent to the silicone rubber / expanded vermiculite prepolymer for cross-linking to form silicone rubber / expanded composite elastomer material. After the expanded vermiculite is doped, the mechanical properties, thermal insulation properties, and flame retardant properties of silicone rubber are improved, but they are far less than the effects of organic flame retardants.
[0006] Patent CN115160645A discloses a method for preparing a vermiculite composite flame retardant material, wherein the vermiculite composite flame retardant material includes vermiculite, carbon nanotubes, boron phosphate, and tin hydroxide. The preparation method of the invention prepares a vermiculite carbon nanotube composite material by pre-treating vermiculite, crystallizing the vermiculite flame retardant material, mixing it with an organic plastic material, and adding a curing agent to obtain a plastic product with high flame retardancy, but the carbon nanotubes are expensive and do not completely solve the limitations of inorganic flame retardants. Summary of the invention
[0007] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a vermiculite-based composite flame retardant and a preparation method thereof, and to prepare the composite flame retardant by using different flame retardant components, and to utilize their synergistic effect and intercalation effect, thereby overcoming the influence of the flame retardant molecules directly dispersed in the material on the material properties in the prior art, and jointly improving the flame retardant and smoke suppression effects of the flame retardant.
[0008] To solve the above problems, the present invention adopts the following technical solutions:
[0009] First, the present invention provides a method for preparing a composite flame retardant based on vermiculite, comprising the following steps:
[0010] (1)Acidified intercalation
[0011] 60-80 parts by weight of nano vermiculite, 8-10 parts by weight of tetramethylammonium bromide and 0.5-2 parts by weight of 98% sulfuric acid are added to 500 parts by weight of deionized water, stirred and reacted at 80°C for 4-8 hours, filtered, washed and dried to obtain vermiculite modified by tetramethylammonium bromide intercalation.
[0012] Before acid intercalation, the layers of vermiculite are tightly fitted. Acid intercalation uses tetramethylammonium bromide to support the tightly bound interlayer structure in an acidic environment. Otherwise, the flame retardant cannot be intercalated directly.
[0013] (2) Particle size flotation
[0014] Take 1 to 8 parts by weight of vermiculite modified by tetramethylammonium bromide intercalation, add 4 to 8 parts by weight of a dispersant, sand grind for 4 to 8 hours using a zirconium oxide ball with a diameter of 2 mm in a sand mill, then add 20 to 30 parts by weight of deionized water, settle for 12 to 24 hours, centrifuge, filter, wash and dry the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers.
[0015] If the particle size range is too wide, small-particle vermiculite or single-piece vermiculite peeled off after acid intercalation will be filled in the interlayers of large-particles, affecting the intercalation effect of the final flame retardant, so the particle size range is between 1μm-100μm.
[0016] (3) Amino coupling
[0017] Add 5-10 parts by weight of the intercalation-modified vermiculite treated in step (2) and 10-15 parts by weight of toluene into a three-necked flask, introduce nitrogen, heat and stir, add 2-8 parts by weight of an aminosilane coupling agent when the temperature rises to 80-100° C., raise the temperature to 120° C. and react for 30 minutes; after the reaction is completed, filter, wash, and vacuum dry to obtain aminated vermiculite.
[0018] Aminosilane coupling agent is added to aminate the hydroxyl groups on the surface and between the layers of vermiculite. Since the reactivity of the H atoms of the amino group is significantly higher than that of the H atoms on the silanol group, the flame retardant intercalation is easier to occur.
[0019] (4) Flame retardant intercalation
[0020] Add 5 to 10 parts by weight of aminated vermiculite and 10 to 15 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 4 to 8 parts by weight of an intercalant when the temperature rises to 40 to 60° C., reflux and stir at 80° C. to react for 0.5 to 1 h, filter, wash, and vacuum dry to obtain an organic-inorganic composite flame retardant based on vermiculite.
[0021] Furthermore, the dispersant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium hexadecyl sulfonate.
[0022] Furthermore, the intercalant is one or more of sodium tripolyphosphate, sodium hexametaphosphate, and sodium borohydride.
[0023] Furthermore, the aminosiloxane coupling agent is one or more of KH550, KH540, KH792, and KH602.
[0024] Secondly, the present invention provides a vermiculite-based composite flame retardant, which is prepared by the above-mentioned preparation method of the vermiculite-based composite flame retardant.
[0025] Thirdly, the vermiculite-based composite flame retardant provided by the present invention is applied to fireproof materials.
[0026] The present invention firstly uses tetramethylammonium bromide to stretch the closely fitted vermiculite interlayers to form a structure with interlayer space, and then adopts a flotation method to obtain vermiculite particles with uniform particle size as much as possible, the purpose of which is to avoid uneven dispersion that may be caused by uneven particle size and affect the intercalation effect of the final flame retardant, and then adopts a silane coupling agent with amino groups to aminate the inside of the vermiculite sheet layer to ensure that the subsequent flame retardant enters the interlayer, that is, better composite. The vermiculite interlayer is a monomolecular hydration layer, each layer of vermiculite is composed of silicon oxygen tetrahedrons, which are connected in an interlayer hydrogen bond mode, and water molecules are also connected to each layer of silicon oxygen tetrahedron in the form of hydrogen bonds. Vermiculite has good dispersibility and compatibility in fire retardant coatings. The present invention intercalates flame retardants such as sodium tripolyphosphate into the vermiculite interlayer, overcoming the shortcomings of poor compatibility between traditional flame retardants and polymers, low adhesion, and poor thermal stability. Vermiculite itself also has excellent flame retardant properties. During the vermiculite flame retardant process, high temperature will cause the vermiculite layers to continue to expand rapidly, which can release flame retardants such as sodium tripolyphosphate. The two work synergistically to achieve better flame retardant performance. DETAILED DESCRIPTION
[0027] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0028] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be purchased from the market.
[0029] Example 1
[0030] (1)Acidified intercalation
[0031] 70 parts by weight of nano vermiculite, 8 parts by weight of tetramethylammonium bromide and 1 part by weight of 98% sulfuric acid are added to 500 parts by weight of deionized water, stirred and reacted at 80° C. for 6 hours, filtered, washed and dried to obtain vermiculite modified by tetramethylammonium bromide intercalation;
[0032] (2) Particle size flotation
[0033] Take 6 parts by weight of tetramethylammonium bromide intercalated modified vermiculite, add 7 parts by weight of sodium hexadecyl sulfate, sand grind for 6 hours using a zirconium oxide ball with a diameter of 2 mm in a sand mill, then add 30 parts by weight of deionized water, settle for 24 hours, obtain a supernatant by decantation, centrifuge, filter, wash and dry the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers;
[0034] (3) Amino coupling
[0035] Add 10 parts by weight of the intercalation-modified vermiculite treated in step (2) and 12 parts by weight of toluene into a three-necked flask, introduce nitrogen, heat and stir, add 6 parts by weight of an aminosilane coupling agent when the temperature reaches 90° C., and heat to 120° C. to react for 30 minutes; after the reaction is completed, filter, wash, and vacuum dry to obtain amination vermiculite;
[0036] (4) Flame retardant intercalation
[0037] Add 8 parts by weight of aminated vermiculite and 12 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 6 parts by weight of sodium tripolyphosphate when the temperature rises to 50°C, reflux and stir at 80°C for 1 hour, filter, wash, and vacuum dry to obtain a vermiculite-based composite flame retardant.
[0038] Example 2
[0039] (1)Acidified intercalation
[0040] 80 parts by weight of nano vermiculite, 10 parts by weight of tetramethylammonium bromide and 2 parts by weight of 98% sulfuric acid are added to 500 parts by weight of deionized water, stirred and reacted at 80° C. for 8 hours, filtered, washed and dried to obtain vermiculite modified by tetramethylammonium bromide intercalation;
[0041] (2) Particle size flotation
[0042] Take 3 parts by weight of tetramethylammonium bromide intercalated modified vermiculite, add 4 parts by weight of sodium dodecylbenzene sulfonate, sand grind for 6 hours with a zirconium oxide ball with a diameter of 2 mm in a sand mill, then add 20 parts by weight of deionized water, settle for 16 hours, centrifuge, filter, wash and dry the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers;
[0043] (3) Amino coupling
[0044] Add 5 parts by weight of the intercalation-modified vermiculite treated in step (2) and 10 parts by weight of toluene into a three-necked flask, introduce nitrogen, heat and stir, add 2 parts by weight of an aminosilane coupling agent when the temperature reaches 80° C., and heat to 120° C. to react for 30 minutes; after the reaction is completed, filter, wash, and vacuum dry to obtain amination vermiculite;
[0045] (4) Flame retardant intercalation
[0046] Add 5 parts by weight of aminated vermiculite and 10 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 4 parts by weight of sodium hexametaphosphate when the temperature rises to 50°C, reflux and stir at 80°C to react for 0.8h, filter, wash, and vacuum dry to obtain a vermiculite-based composite flame retardant.
[0047] Example 3
[0048] (1)Acidified intercalation
[0049] 60 parts by weight of nano vermiculite, 9 parts by weight of tetramethylammonium bromide and 0.8 parts by weight of 98% sulfuric acid are added to 500 parts by weight of deionized water, stirred and reacted at 80° C. for 4 hours, filtered, washed and dried to obtain vermiculite modified by tetramethylammonium bromide intercalation;
[0050] (2) Particle size flotation
[0051] Take 8 parts by weight of tetramethylammonium bromide intercalated modified vermiculite, add 8 parts by weight of sodium dodecyl sulfate, sand grind for 8 hours with a zirconium oxide ball with a diameter of 2 mm in a sand mill, then add 30 parts by weight of deionized water, settle for 20 hours, centrifuge, filter, wash and dry the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers;
[0052] (3) Amino coupling
[0053] Add 5-10 parts by weight of the intercalation-modified vermiculite treated in step (2) and 10-15 parts by weight of toluene into a three-necked flask, introduce nitrogen, heat and stir, add 2-8 parts by weight of an aminosilane coupling agent when the temperature rises to 80-100° C., raise the temperature to 120° C. and react for 30 minutes; after the reaction is completed, filter, wash, and vacuum dry to obtain amination vermiculite;
[0054] (4) Flame retardant intercalation
[0055] Add 10 parts by weight of aminated vermiculite and 15 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 8 parts by weight of sodium borohydride when the temperature rises to 60°C, reflux and stir to react at 80°C for 1 hour, filter, wash, and vacuum dry to obtain a vermiculite-based composite flame retardant.
[0056] Comparative Example 1
[0057] (1) adding 70 parts by weight of nano-vermiculite, 8 parts by weight of tetramethylammonium bromide and 1 part by weight of 98% sulfuric acid to 500 parts by weight of deionized water, stirring and reacting at 80° C. for 6 hours, filtering, washing and drying to obtain vermiculite modified by tetramethylammonium bromide intercalation;
[0058] (2) taking 6 parts by weight of tetramethylammonium bromide intercalated modified vermiculite, adding 7 parts by weight of sodium hexadecyl sulfate, sand milling for 6 hours using a zirconium oxide ball with a diameter of 2 mm in a sand mill, adding 30 parts by weight of deionized water, settling for 24 hours, obtaining a supernatant by decantation, centrifuging, filtering, washing, and drying the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers;
[0059] (3) Add 10 parts by weight of the intercalation-modified vermiculite treated in step (2) and 12 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 6 parts by weight of sodium tripolyphosphate when the temperature rises to 50° C., reflux and stir at 80° C. for 1 h, filter, wash, and vacuum dry to obtain a vermiculite-based composite flame retardant.
[0060] Comparative Example 2
[0061] (1) adding 70 parts by weight of nano-vermiculite, 8 parts by weight of tetramethylammonium bromide and 1 part by weight of 98% sulfuric acid to 500 parts by weight of deionized water, stirring and reacting at 80° C. for 6 hours, filtering, washing and drying to obtain vermiculite modified by tetramethylammonium bromide intercalation;
[0062] (2) Take 6 parts by weight of vermiculite modified by tetramethylammonium bromide intercalation and 6 parts by weight of sodium tripolyphosphate, add 7 parts by weight of sodium hexadecyl sulfate, and sand grind them in a sand mill with a zirconium oxide ball with a diameter of 2 mm for 6 hours, then add 30 parts by weight of deionized water, settle for 24 hours, and obtain the supernatant by decantation. The supernatant is centrifuged, filtered, washed, and dried to obtain a vermiculite-based composite flame retardant.
[0063] Comparative Example 3
[0064] The nano-vermiculite and sodium tripolyphosphate were ground in a ball mill in a weight ratio of 1:1, and then sieved to 200 meshes to obtain a composite flame retardant.
[0065] In the material tank of the high-speed disperser, 50 parts by weight of water are added. Under high-speed dispersion, 0.4 parts by weight of dispersant 5040, 0.4 parts by weight of defoamer NXZ, and 0.4 parts by weight of wetting agent OP-10 are added in sequence, and then 100.0 parts by weight of the intumescent examples 1-3 and comparative examples 1-3 are slowly added to obtain the composite flame retardant. The mixture is dispersed at high speed for 2 hours, the dispersion speed is reduced, 25.0 parts by weight of polyacrylate emulsion and an appropriate amount of polyacrylic acid thickener, pH adjuster AMP-95, etc. are added, and the mixture is stirred and dispersed for more than 1 hour to obtain a fire retardant coating.
[0066] The fire retardant coatings made of the composite flame retardants prepared in Examples 1-3 and Comparative Examples 1-3 were tested and evaluated. The test results are shown in Table 1.
[0067] (1) Flame retardant performance: According to UL94 standard, vertical combustion test was carried out on it.
[0068] (2) Limiting oxygen index: tested in accordance with GBT 2406.2 standard.
[0069] (3) Smoke density: tested in accordance with GB / T 8323.2.
[0070] (4) Adhesion test: refer to GB / T9286-1998.
[0071] (5) Constant temperature and humidity weathering test: The paint film was cured on an IPC B 25A comb-type electrode plate with a dry film thickness of 50 μm and placed in a constant temperature and humidity chamber at 85°C and 85% RH for 720 h. After the test, the paint film was observed for white spots, blistering, pinholes, cracks, fine cracks, wrinkles, shedding, separation, discoloration and other surface phenomena.
[0072] (6) Hot and cold shock test: The paint film was cured on an IPC B 25A comb-type electrode plate with a dry film thickness of 50 μm. The film was placed in an environmental test chamber with a high temperature of 125°C and a low temperature of 40°C. The high and low temperature holding time was 30 minutes each, and the high and low temperature switching time was 2 minutes. The test was repeated for 700 cycles.
[0073] (7) Salt spray resistance test: GB / T 1771-1991 Determination of the neutral salt spray resistance of paints and varnishes; after the test, observe the appearance of the paint film for blistering, rust, creep, whitening, blackening, shedding, separation, etc.
[0074] Table 1
[0075]
[0076] It can be seen from the data in Table 1 that, first, sodium tripolyphosphate and other flame retardants are intercalated between the vermiculite layers, and the vermiculite itself also has excellent flame retardant properties. During the vermiculite flame retardant process, high temperature will allow the vermiculite layers to continue to expand sharply, so that sodium tripolyphosphate and other flame retardants can be released. The two are flame retardant in a coordinated manner, and have more excellent flame retardant performance. Secondly, the vermiculite interlayer of the present invention is a monomolecular hydration layer, and each layer of vermiculite is composed of silicon oxygen tetrahedrons, which are connected in an interlayer hydrogen bond manner. Water molecules are also connected to each layer of silicon oxygen tetrahedron in the form of hydrogen bonds. Vermiculite has good dispersibility and compatibility in fire retardant coatings. The present invention intercalates sodium tripolyphosphate and other flame retardants between the vermiculite layers, overcoming the shortcomings of poor compatibility of traditional flame retardants with polymers, low adhesion, and poor thermal stability.
[0077] According to the disclosure of the above description, those skilled in the art to which the present invention belongs may also make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A method for preparing a composite flame retardant based on vermiculite, characterized in that: The steps include: (1)Acidified intercalation 60-80 parts by weight of nano vermiculite, 8-10 parts by weight of tetramethylammonium bromide and 0.5-2 parts by weight of 98% sulfuric acid are added to 500 parts by weight of deionized water, stirred at 80° C. for 4-8 hours, filtered, washed and dried to obtain vermiculite modified by tetramethylammonium bromide intercalation; (2) Particle size flotation Take 1 to 8 parts by weight of vermiculite modified by tetramethylammonium bromide intercalation, add 4 to 8 parts by weight of a dispersant, sand grind for 4 to 8 hours using a zirconium oxide ball with a diameter of 2 mm in a sand mill, then add 20 to 30 parts by weight of deionized water, settle for 12 to 24 hours, centrifuge, filter, wash and dry the supernatant to obtain vermiculite with uniform particle size and containing tetramethylammonium bromide between layers; (3) Amino coupling Add 5-10 parts by weight of the intercalation-modified vermiculite treated in step (2) and 10-15 parts by weight of toluene into a three-necked flask, introduce nitrogen, heat and stir, add 2-8 parts by weight of an aminosilane coupling agent when the temperature rises to 80-100° C., raise the temperature to 120° C. and react for 30 minutes; after the reaction is completed, filter, wash, and vacuum dry to obtain amination vermiculite; (4) Flame retardant intercalation Add 5 to 10 parts by weight of aminated vermiculite and 10 to 15 parts by weight of ethanol into a three-necked flask, introduce nitrogen, heat and stir, add 4 to 8 parts by weight of an intercalant when the temperature rises to 40 to 60° C., reflux and stir at 80° C. for 0.5 to 1 hour, filter, wash, and vacuum dry to obtain a vermiculite-based composite flame retardant; the intercalant is one or more of sodium tripolyphosphate, sodium hexametaphosphate, and sodium borohydride.
2. The method for preparing a composite flame retardant based on vermiculite according to claim 1, characterized in that: The dispersant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and sodium hexadecyl sulfonate.
3. The method for preparing a composite flame retardant based on vermiculite according to claim 1, characterized in that: The aminosiloxane coupling agent is one or more of KH550, KH540, KH792 and KH602.
4. A composite flame retardant based on vermiculite, characterized in that: The composite flame retardant is prepared by the method for preparing the vermiculite-based composite flame retardant according to any one of claims 1 to 3.
5. The vermiculite-based composite flame retardant according to claim 4, characterized in that: The composite flame retardant is used in fireproof materials.