A method and system for pyrolysis recovery of waste plastics
Through the preliminary melting, liquefaction, dechlorination and pyrolysis treatment of chlorine-containing waste plastics, combined with the mixing reaction of high-temperature pyrolysis raw materials, the problems of furnace tube coking and chlorine removal are solved, and the resource utilization and green recycling of waste plastics are realized.
Patent Information
- Application Number
- CN202111276209.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing technology is difficult to effectively process chlorine-containing waste plastics, resulting in the coking of furnace tubes during the heating process of liquefied waste plastic oil, and the inability to efficiently remove chlorine from waste plastics, which limits the resource utilization of waste plastics.
Through preliminary melting, liquefaction and dechlorination treatment of chlorine-containing waste plastics, a transportable fluid is formed, and then mixed with high-temperature pyrolysis raw materials to enter the pyrolysis reaction to generate pyrolysis gas, liquid fraction and a small amount of coke, thereby realizing the resource utilization of waste plastics. And avoid the problem of furnace tube coking during the heating process of liquefied waste plastic oil.
It achieves efficient dechlorination and resource utilization of waste plastics, avoids furnace tube coking, has a simple process flow, requires less equipment investment, and achieves green resource recycling.
Smart Images

Figure CN116064064B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of waste plastic resource recycling and processing, and in particular, to a method and system for pyrolysis recovery of waste plastics. Background Art
[0002] With the advancement of science and technology and industrial development, plastics are widely used as packaging materials in people's daily lives. Used waste plastics cannot be decomposed by themselves in nature. Only a few types of waste plastics can be reprocessed and reused through specific recycling channels. A large amount of waste plastics enters landfills in the form of domestic garbage. Since waste plastics are not easy to decompose, they occupy a lot of space. In recent years, the amount of waste plastics has increased rapidly. It has become an urgent task to recycle waste plastics quickly and greenly.
[0003] The simplest chemical method to deal with waste plastics is direct incineration, but direct incineration will produce toxic gases such as dioxins that are harmful to the human body, causing secondary environmental pollution. Waste plastic oil technology is to pyrolyze waste plastics under anaerobic or anoxic conditions by heating or with a catalyst, so that polymers are pyrolyzed into low molecular substances to obtain gasoline, kerosene, diesel fractions and some pyrolysis gases. On the one hand, waste plastic oil technology alleviates the pollution problem caused by waste plastics, and on the other hand, it realizes the recycling of waste plastics, which is an important direction for the resource treatment of waste plastics.
[0004] At present, waste plastic oil recovery technologies mainly include waste plastic pyrolysis, catalytic pyrolysis and pyrolysis-catalytic modification technology. Pyrolysis has the advantages of simple process, relatively less equipment investment, no need for catalyst, and short reaction process, making the pyrolysis method the lowest unit oil cost compared to the other two technologies. General waste plastics in domestic garbage undergo high-temperature pyrolysis reaction between 380 and 500°C, with a fast pyrolysis rate and a relatively simple product composition, which can be used as oil products or chemical raw materials.
[0005] CN109401774A discloses a waste plastic continuous pyrolysis system and a pyrolysis method thereof, the system comprises a loading device, a feeding device, a pyrolysis reactor and a slag discharge device connected in sequence, and because the plastic is a macromolecular polymer, a non-Newtonian fluid is formed during the heating process, and a screw propeller is used. The plastic liquefaction process in this process is subjected to uneven heating, which is prone to coking and fouling.
[0006] CN10461030B discloses a coking method for producing fuel oil from waste plastics. The method comprises the following steps: preheating high aromatic components and waste plastics or plastic oil in a raw material buffer tank, and then heating them in a tubular heating furnace, and then spraying them into a delayed coking tower for coking reaction. The waste plastics mentioned in the method are one or more of polyethylene, polypropylene and polystyrene, and do not contain polyvinyl chloride (PVC). Therefore, the method cannot process waste plastic raw materials mixed with polyvinyl chloride (PVC).
[0007] CN112538363A discloses a method for co-converting waste plastics in a delayed coker unit, wherein the waste plastics are converted together with petroleum residue raw materials, wherein the waste plastics are selected from polyethylene, polypropylene, polystyrene, PET and multi-layer plastics with metal added, and also do not include waste plastics of polyvinyl chloride (PVC). The waste plastics form a high-viscosity polymer melt during the melting process, and there is a density difference problem with the hydrocarbon raw material, so the mixed fluid of the hydrocarbon and polymer melt can cause problems such as blockage and coking of the delayed coking heating furnace tube. Summary of the invention
[0008] The purpose of the present disclosure is to provide a method and system for pyrolysis recovery of waste plastics, which can avoid the coking problem of furnace tubes during the heating process of liquefied waste plastic oil and achieve efficient removal of chlorine in waste plastics; and recover waste plastics through pyrolysis reaction to achieve resource utilization of waste plastics.
[0009] Through the above technical scheme, the first aspect of the present disclosure provides a method for pyrolysis recovery of waste plastics, comprising the following steps: S1, allowing chlorine-containing waste plastics to enter a waste plastic preliminary melting and liquefaction dechlorination unit for hot melt dechlorination treatment to obtain a gaseous material containing hydrogen chloride and a dechlorinated waste plastic liquid material; S2, allowing the dechlorinated waste plastic liquid material and a high-temperature pyrolysis raw material to enter a material mixing unit for mixing, respectively, to obtain a mixed pyrolysis raw material; S3, allowing the mixed pyrolysis raw material to enter a pyrolysis reaction unit for pyrolysis, to obtain a pyrolysis gaseous product and coke; S4, allowing the pyrolysis gaseous product to enter a separation unit for separation, to obtain dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction.
[0010] Optionally, the method further comprises: allowing the dechlorinated waste plastic liquid phase material obtained in step S1 to enter a high-temperature liquefaction unit for heat treatment to obtain high-temperature liquefied waste plastic; then allowing the high-temperature liquefied waste plastic to enter the material mixing unit; preferably, the high-temperature liquefaction unit comprises a second screw pump, and the dechlorinated waste plastic liquid phase material is subjected to the heat treatment in the second screw pump; the conditions for the heat treatment include: an outlet temperature of 400 to 500°C, preferably 430 to 450°C.
[0011] Optionally, the method further comprises: allowing the pyrolysis raw material to enter a heating unit for heating to obtain the high-temperature pyrolysis raw material; preferably, the temperature of the high-temperature pyrolysis raw material is 480°C to 650°C, preferably 500°C to 600°C.
[0012] Optionally, in step S2, the weight ratio of the high-temperature pyrolysis raw material to the chlorine-containing waste plastic is 0.1 to 10:1, preferably 0.3 to 5:1.
[0013] Optionally, the pyrolysis feedstock includes hydrocarbon oil; the hydrocarbon oil is selected from one or more of heavy crude oil, acidic crude oil, atmospheric residue, vacuum wax oil, coker wax oil, deasphalted oil, hydrocracking tail oil, coal tar, shale oil, tank bottom oil, coal liquefaction residual oil or other secondary processed distillate oil; optionally, the method also includes: before entering the heating unit, allowing the hydrocarbon oil to enter the bottom of the tower of the separation unit for preliminary preheating.
[0014] Optionally, tail oil can be obtained after separation by the separation unit; the pyrolysis feedstock includes an external pyrolysis feedstock and optional circulating oil, and the circulating oil includes the wax oil fraction, the tail oil and the optional diesel fraction separated from the separation unit; the method also includes: allowing the external pyrolysis feedstock to enter the heating unit for heating and then enter the material mixing unit as the high-temperature pyrolysis feedstock; or allowing the circulating oil to enter the heating unit for heating and then enter the material mixing unit as the high-temperature pyrolysis feedstock; or allowing the circulating oil and the external pyrolysis feedstock to enter the heating unit together for heating, and then allowing the heated mixture to enter the material mixing unit as the high-temperature pyrolysis feedstock; optionally, the weight ratio of the circulating oil to the chlorine-containing waste plastic is 0.2 to 5.0, preferably 0.2 to 2.
[0015] Optionally, in step S1, the waste plastic preliminary melting, liquefaction and dechlorination unit comprises a first screw pump and a vacuum device connected to the first screw pump, and the conditions of the hot melt dechlorination treatment include: an outlet temperature of 200 to 430° C., preferably 300 to 375° C.; and a vacuum degree of the waste plastic preliminary melting, liquefaction and dechlorination unit (1) of 1 to 650 mmHg, preferably 100 to 400 mmHg.
[0016] Optionally, the chlorine-containing waste plastics include PVC and other plastics, and the other plastics are selected from one or more of LDPE, HDPE, PS, and PP; the content of the PVC is less than 10 weight %. Optionally, the ash content of the chlorine-containing waste plastics is less than 25 weight %.
[0017] Optionally, the pyrolysis reaction unit comprises a pyrolysis tower, the pressure at the top of the pyrolysis tower is 0.05-0.6 MPa, preferably 0.1-0.3 MPa, and the pyrolysis reaction temperature is 400-550°C, preferably 430-480°C.
[0018] Optionally, the method further comprises: allowing the gaseous material containing hydrogen chloride obtained by the dechlorination unit of the preliminary melting and liquefaction of the waste plastic to enter the gaseous dechlorination unit under the suction action of the vacuum device, and contacting with a hydrogen chloride absorbent to perform hydrogen chloride absorption treatment; introducing the gaseous phase after the hydrogen chloride absorption treatment and the dry gas separated by the separation unit into a subsequent treatment device; optionally, the hydrogen chloride absorbent is water or an alkali solution with a pH greater than 7, and the alkali solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution and ammonia water.
[0019] According to a second aspect of the present disclosure, there is provided a system for recycling waste plastics by pyrolysis, which comprises: a waste plastics preliminary melting, liquefaction and dechlorination unit, a material mixing unit, a pyrolysis reaction unit and a separation unit; the waste plastics preliminary melting, liquefaction and dechlorination unit is provided with a chlorine-containing waste plastics inlet, a first screw pump, a hydrogen chloride-containing gas phase outlet and a dechlorinated waste plastics liquid phase material outlet; the chlorine-containing waste plastics inlet is used to introduce waste plastic raw materials; the material mixing unit is provided with a dechlorinated waste plastics inlet, a high-temperature pyrolysis raw material inlet and a mixed pyrolysis raw material outlet, and the dechlorinated waste plastics inlet is connected to the dechlorinated waste plastics liquid phase material outlet of the waste plastics preliminary melting, liquefaction and dechlorination unit; the pyrolysis reaction unit is provided with a mixed pyrolysis raw material inlet, a pyrolysis tower and a pyrolysis product outlet; the mixed pyrolysis raw material inlet of the pyrolysis reaction unit is connected to the mixed pyrolysis raw material outlet of the material mixing unit; the separation unit is provided with a material inlet to be separated, a fractionating tower, a dry gas and liquefied gas outlet, a gasoline fraction, a diesel fraction outlet, a wax oil fraction outlet and a tail oil outlet; the material inlet to be separated of the separation unit is connected to the pyrolysis product outlet of the pyrolysis reaction unit.
[0020] Optionally, the system further comprises a high-temperature liquefaction unit and a heating unit; the high-temperature liquefaction unit comprises an inlet for plastic to be heated, a second screw pump and an outlet for high-temperature liquefied plastic; the heated plastic inlet of the high-temperature liquefaction unit is connected to the outlet for liquid phase material of dechlorinated waste plastic of the waste plastic preliminary melting and liquefaction dechlorination unit, and the high-temperature liquefied plastic outlet of the high-temperature liquefaction unit is connected to the inlet for dechlorinated waste plastic of the material mixing unit; optionally, the heating unit comprises a pyrolysis raw material heating inlet and a high-temperature pyrolysis raw material outlet, and the pyrolysis raw material heating inlet of the heating unit is used to introduce the pyrolysis raw material to be heated, The high-temperature pyrolysis feedstock outlet of the heating unit is connected to the high-temperature pyrolysis feedstock inlet of the material mixing unit; optionally, the pyrolysis feedstock heating inlet of the heating unit is also connected to the wax oil fraction outlet, the diesel fraction outlet and the tail oil outlet of the separation unit respectively; optionally, a fresh pyrolysis feedstock preheating inlet and a preheated fresh feedstock outlet are provided at the bottom of the separation unit; the fresh pyrolysis feedstock preheating inlet of the separation unit is used to introduce pyrolysis feedstock oil; the preheated fresh feedstock outlet of the separation unit is connected to the pyrolysis feedstock heating inlet of the heating unit; or the pyrolysis feedstock heating inlet of the heating unit is directly connected to the fresh pyrolysis feedstock source through a pipeline for introducing fresh pyrolysis feedstock oil; optionally, the system also includes a gas phase dechlorination unit, the gas phase dechlorination unit includes a gas phase material inlet containing hydrogen chloride, a treated gas phase material outlet and a hydrogen chloride absorbent; the gas phase material inlet containing hydrogen chloride of the gas phase dechlorination unit is connected to the gas phase outlet containing hydrogen chloride through a vacuum system; optionally, the pyrolysis reaction unit includes a plurality of pyrolysis reaction devices arranged in parallel.
[0021] Through the above technical scheme, the present disclosure provides a method and system for pyrolysis recovery of waste plastics. The present disclosure preliminarily liquefies and dechlorinates waste plastics by heating to form a transportable fluid. After dechlorination, the waste plastics are further heated and mixed with high-temperature recycled oil heated by a heating furnace, and then enter a pyrolysis tower for pyrolysis reaction to generate pyrolysis gas, liquid fractions and a small amount of coke, etc., to achieve resource utilization of waste plastics, and can also avoid the coking phenomenon of furnace tubes during the heating process of liquefied waste plastic oil. The present disclosure has a simple process flow and relatively less equipment investment, so that waste plastics can be recycled in a green resource manner.
[0022] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0024] Figure 1A process flow chart of the method for pyrolysis recovery of waste plastics provided in the present invention.
[0025] Description of Reference Numerals
[0026] 1-Waste plastics preliminary melting, liquefaction and dechlorination unit, 2-High temperature liquefaction unit, 3-Material mixing unit, 4-Gas phase dechlorination unit, 5-Pyrolysis reaction unit, 6-Separation unit, 7-Heating unit, 8-Chlorine-containing waste plastics, 9-Pipeline, 10-Pipeline, 11-Pipeline, 12-Pipeline, 13-Pipeline, 14-Pipeline, 15-Pipeline, 16-Pipeline, 17-Pipeline, 18-Pipeline, 19-Pipeline, 20-Pipeline DETAILED DESCRIPTION
[0027] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0028] In the present disclosure, unless otherwise stated, the words "first", "second", "third", etc. are used only to distinguish different components and do not have actual meanings such as the order of connection between the front and the back. In the present disclosure, the directional words used, such as "upper, lower, top, bottom", usually refer to the upper and lower, top and bottom of the device in normal use. "Inside and outside" refer to the outline of the device.
[0029] The first aspect of the present disclosure provides a method for pyrolysis recovery of waste plastics, such as Figure 1 As shown, the following steps are included:
[0030] S1, allowing the chlorine-containing waste plastics to enter the waste plastics preliminary melting and liquefaction dechlorination unit separation unit 1 separation unit for hot melt dechlorination treatment to obtain a gas phase material containing hydrogen chloride and a dechlorinated waste plastic liquid phase material;
[0031] S2, allowing the dechlorinated waste plastic liquid phase material and the high-temperature pyrolysis raw material to enter the material mixing unit separation unit 3 separation unit for mixing to obtain a mixed pyrolysis raw material;
[0032] S3, allowing the mixed pyrolysis raw material to enter the pyrolysis reaction unit separation unit 5 separation unit for pyrolysis to obtain pyrolysis gaseous products and coke;
[0033] S4, allowing the pyrolysis gaseous product to enter the separation unit 6 for separation to obtain dry gas and liquefied gas, gasoline fraction, diesel fraction and wax oil fraction.
[0034] The present invention preliminarily liquefies and dechlorinates waste plastics by heating to form a transportable fluid. The dechlorinated waste plastics are further heated and mixed with high-temperature recycled oil or fresh raw material source heated by a heating furnace, and then enter a pyrolysis tower for pyrolysis reaction to generate pyrolysis gas, liquid fractions and a small amount of coke, etc., thereby realizing resource utilization of waste plastics and avoiding the coking phenomenon of furnace tubes during the heating process of liquefied waste plastic oil.
[0035] In a specific embodiment, the chlorine-containing waste plastics include PVC and other plastics, and the other plastics are selected from one or more of LDPE, HDPE, PS, and PP; the content of the PVC is less than 10% by weight, and optionally, the ash content of the chlorine-containing waste plastics is less than 25% by weight. The present disclosure is applicable to a wide range of waste plastic raw materials.
[0036] In a specific embodiment, the high-temperature pyrolysis feedstock can be an external hydrocarbon oil, or a circulating oil from the pyrolysis product in the system, or both.
[0037] In one embodiment, if Figure 1 As shown, the method further includes: allowing the dechlorinated waste plastic liquid phase material obtained in step S1 to enter the high temperature liquefaction unit 2 for heating treatment to obtain high temperature liquefied waste plastic; and then allowing the high temperature liquefied waste plastic to enter the material mixing unit 3. In the present disclosure, the dechlorinated waste plastic liquid phase material enters the high temperature liquefaction unit to further increase the temperature and reduce the viscosity.
[0038] In a preferred embodiment, the high-temperature liquefaction unit 2 includes a second screw pump, and the dechlorinated waste plastic liquid phase material is subjected to the heating treatment in the second screw pump; the conditions of the heating treatment include: an outlet temperature of 400-500°C, preferably 430-450°C.
[0039] In one embodiment, if Figure 1 As shown, the method further includes: allowing the pyrolysis raw material to enter the heating unit 7 for heating to obtain the high-temperature pyrolysis raw material;
[0040] Preferably, the temperature of the high-temperature pyrolysis raw material is 480°C to 650°C, preferably 500°C to 600°C; the heating unit 7 is a heating furnace, and the water vapor injection amount of the heating furnace is 0.5 to 5% by weight, preferably 1 to 3% by weight, based on the total weight of the material introduced into the heating furnace.
[0041] The present invention heats the pyrolysis raw material in the heating unit to a temperature higher than the outlet temperature of the waste plastic high-temperature liquefaction unit 2, so that the high-temperature pyrolysis raw material and the high-temperature liquefied waste plastic can be heat-exchanged at the temperature of the high-temperature pyrolysis raw material itself during the mixing process in the material mixing unit 3.
[0042] In a specific embodiment, the pyrolysis feedstock includes hydrocarbon oil; the hydrocarbon oil is selected from one or more of heavy crude oil, acidic crude oil, atmospheric residue oil, vacuum wax oil, coker wax oil, deasphalted oil, hydrocracking tail oil, coal tar, shale oil, tank bottom oil, coal liquefaction residual oil or other secondary processed distillate oils.
[0043] In an optional implementation, if Figure 1 As shown, the method further includes: before entering the heating unit 7, the hydrocarbon oil is allowed to enter the bottom of the tower of the separation unit 6 for preliminary preheating. The heat utilization efficiency of the devices in the system is improved. In another embodiment, the hydrocarbon oil may not enter the bottom of the tower of the separation unit 6 for preheating, but is directly introduced into the heating unit for heating. The separation unit in the present disclosure can adopt a device conventionally selected in the art, such as a fractionation tower.
[0044] In one embodiment, in step S2, the weight ratio of the high-temperature pyrolysis raw material to the chlorine-containing waste plastic is 0.1 to 10:1, preferably 0.3 to 5:1.
[0045] In one embodiment, the separation unit 6 can also obtain tail oil after separation; the pyrolysis feedstock includes external pyrolysis feedstock and optional circulating oil, and the circulating oil includes the wax oil fraction, the tail oil and the optional diesel fraction separated from the separation unit 6; the method further includes:
[0046] Allowing the external pyrolysis raw material to enter the heating unit 7 for heating and then enter the material mixing unit 3 as the high-temperature pyrolysis raw material; or
[0047] The circulating oil is heated in the heating unit 7 and then enters the material mixing unit 3 as the high-temperature pyrolysis raw material; or
[0048] After the circulating oil and the external pyrolysis raw material are jointly introduced into the heating unit 7 for heating, the heated mixed material is introduced into the material mixing unit 3 as the high-temperature pyrolysis raw material.
[0049] In one embodiment, when the circulating oil obtained from the separation unit is introduced into the material mixing unit 3, the weight ratio of the circulating oil to the chlorinated waste plastic is 0.2:1 to 5.0:1, preferably 0.2:1 to 2:1. The present disclosure uses the wax oil fraction, tail oil and optional diesel fraction obtained by product separation as circulating materials, mixes them with the added fresh pyrolysis raw materials, and then heats them in a heating furnace and mixes them together with the dechlorinated waste plastic liquid phase material, which is beneficial to increase the temperature of the waste plastic to the pyrolysis reaction temperature and enter the pyrolysis tower for pyrolysis reaction; directly heating the liquefied waste plastic oil without using a heating furnace avoids the problem of coking of the furnace tubes during the heating process of the liquefied waste plastic; and the recycling of circulating materials can further improve resource utilization.
[0050] In a specific implementation manner, Figure 1 As shown, fresh hydrocarbon oil (external pyrolysis raw material) and optional diesel fraction can be directly mixed with the wax oil fraction, and then mixed with the tail oil introduced through the bottom of the separation unit, and introduced together into the heating unit 7 for heating; then the heated circulating oil and hydrocarbon oil mixture are introduced together into the material mixing unit 3.
[0051] In one embodiment, in step S1, the waste plastic preliminary melting and liquefaction dechlorination unit 1 includes a first screw pump and a vacuum device connected to the first screw pump, and the conditions of the hot melt dechlorination treatment include: the outlet temperature is 200-430°C, preferably 300-375°C; the vacuum degree of the waste plastic preliminary melting and liquefaction dechlorination unit 1 is 1-650 mmHg, preferably 100-400 mmHg. The inventors of the present disclosure have found in experiments that by adopting the dechlorination conditions provided in this embodiment, when a mixture containing multiple waste plastics is treated in the first screw pump, the PVC-containing waste plastic can be firstly pyrolyzed without pyrolysis of other types of plastics, and then the HCl product can be quickly separated by using a vacuum system, thereby improving the dechlorination rate of the waste plastics.
[0052] In one embodiment, if Figure 1 As shown, the method also includes:
[0053] The gaseous material containing hydrogen chloride obtained by the dechlorination unit 1 of the preliminary melting and liquefaction of the waste plastic enters the gaseous dechlorination unit 4 under the suction action of the vacuum device, and contacts with the hydrogen chloride absorbent to carry out hydrogen chloride absorption treatment; the gaseous phase after the hydrogen chloride absorption treatment and the dry gas separated by the separation unit 6 are introduced into a subsequent treatment device together;
[0054] Optionally, the hydrogen chloride absorbent is water or an alkali solution with a pH greater than 7, and the alkali solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution and ammonia water.
[0055] In one embodiment, the pyrolysis reaction unit 5 comprises a pyrolysis tower, the pressure at the top of the pyrolysis tower is 0.05-0.6 MPa, preferably 0.1-0.3 MPa, and the pyrolysis reaction temperature is 400-550° C., preferably 430-480° C. The pyrolysis tower can be a device conventionally selected in the art.
[0056] In a specific implementation manner, Figure 1 As shown, the present disclosure adopts two pyrolysis towers arranged in parallel. According to the actual process, the two pyrolysis towers can be switched according to the amount of coke in the pyrolysis tower. Specifically, the pyrolysis material can be first introduced into one of the pyrolysis towers for reaction. As the reaction proceeds, the amount of coke in the pyrolysis tower gradually increases; when the coke accumulates to a certain amount and needs to be removed from the tower, the introduction of the material into the pyrolysis tower is stopped, and the material is introduced into another pyrolysis tower to continue the reaction, and the coke in the stopped pyrolysis tower is discharged.
[0057] The second aspect of the present disclosure provides a system for pyrolysis recovery of waste plastics, such as Figure 1 As shown, the system comprises: a waste plastic preliminary melting, liquefaction and dechlorination unit 1, a material mixing unit 3, a pyrolysis reaction unit 5 and a separation unit 6;
[0058] The waste plastic preliminary melting, liquefaction and dechlorination unit 1 is provided with a chlorine-containing waste plastic inlet, a first screw pump, a hydrogen chloride-containing gas phase outlet and a dechlorinated waste plastic liquid phase material outlet; the chlorine-containing waste plastic inlet is used to introduce waste plastic raw materials;
[0059] The material mixing unit 3 is provided with a dechlorinated waste plastic inlet, a high-temperature pyrolysis raw material inlet and a mixed pyrolysis raw material outlet, and the dechlorinated waste plastic inlet is connected to the dechlorinated waste plastic liquid phase material outlet of the waste plastic preliminary melting and liquefaction dechlorination unit 1;
[0060] The pyrolysis reaction unit 5 is provided with a mixed pyrolysis raw material inlet, a pyrolysis tower and a pyrolysis product outlet; the mixed pyrolysis raw material inlet of the pyrolysis reaction unit 5 is connected to the mixed pyrolysis raw material outlet of the material mixing unit 3;
[0061] The separation unit 6 is provided with an inlet for materials to be separated, a fractionating tower, outlets for dry gas and liquefied gas, outlets for gasoline fraction, diesel fraction, wax oil fraction and tail oil; the inlet for materials to be separated of the separation unit 6 is connected with the pyrolysis product outlet of the pyrolysis reaction unit 5.
[0062] In one embodiment, if Figure 1As shown, the system further includes a high-temperature liquefaction unit 2 and a heating unit 7; the high-temperature liquefaction unit 2 includes an inlet for the plastic to be heated, a second screw pump and an outlet for the high-temperature liquefied plastic; the heated plastic inlet of the high-temperature liquefaction unit 2 is connected to the outlet of the dechlorinated waste plastic liquid phase material of the waste plastic preliminary melting and liquefaction dechlorination unit 1, and the high-temperature liquefied plastic outlet of the high-temperature liquefaction unit 2 is connected to the inlet of the dechlorinated waste plastic of the material mixing unit 3;
[0063] Optionally, the heating unit 7 includes a pyrolysis raw material heating inlet and a high-temperature pyrolysis raw material outlet, the pyrolysis raw material heating inlet of the heating unit 7 is used to introduce the pyrolysis raw material to be heated, and the high-temperature pyrolysis raw material outlet of the heating unit 7 is connected to the high-temperature pyrolysis raw material inlet of the material mixing unit 3;
[0064] Optionally, the pyrolysis feedstock heating inlet of the heating unit 7 is also connected to the wax oil fraction outlet, the diesel fraction outlet and the tail oil outlet of the separation unit 6 respectively;
[0065] Optionally, a fresh pyrolysis feedstock preheating inlet and a preheated fresh feedstock outlet are provided at the bottom of the separation unit 6; the fresh pyrolysis feedstock preheating inlet of the separation unit 6 is used to introduce pyrolysis feedstock oil; the preheated fresh feedstock outlet of the separation unit 6 is connected to the pyrolysis feedstock heating inlet of the heating unit 7; or the pyrolysis feedstock heating inlet of the heating unit 7 is directly connected to the fresh pyrolysis feedstock source through a pipeline for introducing fresh pyrolysis feedstock oil.
[0066] In one embodiment, if Figure 1 As shown, the system further includes a gas phase dechlorination unit 4, which includes a gas phase material inlet containing hydrogen chloride, a treated gas phase material outlet and a hydrogen chloride absorbent; the gas phase material inlet containing hydrogen chloride and the gas phase outlet containing hydrogen chloride of the gas phase dechlorination unit 4 are connected through a vacuum system;
[0067] Optionally, the pyrolysis reaction unit 5 includes a plurality of pyrolysis reaction devices arranged in parallel.
[0068] Using this disclosure Figure 1 The system shown in the figure performs pyrolysis to recycle waste plastics, including the following processes:
[0069] The chlorine-containing waste plastic 8 enters the waste plastic preliminary melting, liquefaction and dechlorination unit 1, where it is mixed, melted and dechlorinated. The gaseous material containing hydrogen chloride quickly enters the gaseous phase dechlorination unit 4 through the vacuum system to contact with the hydrogen chloride absorbent to absorb hydrogen chloride. The absorption liquid obtained by absorbing hydrogen chloride is discharged through pipeline 20. A small amount of cracked gas (the waste plastic inevitably cracks under heating conditions in the waste plastic preliminary melting, liquefaction and dechlorination unit 1) is mixed with the gas (dry gas and liquefied gas) separated from the distillation tower through pipeline 18 and led out through pipeline 19; dechlorination The melted dechlorinated waste plastic (dechlorinated waste plastic liquid phase material) enters the high-temperature liquefaction unit 2, where the liquefied dechlorinated waste plastic is heated to further increase the temperature and reduce the viscosity to obtain high-temperature liquefied waste plastic. The high-temperature liquefied waste plastic, together with the high-temperature circulating oil obtained by heating the heating unit 7 (heating furnace) from the pipeline 17 and the high-temperature pyrolysis raw material, enter the material mixing unit 3, where the material reaches the reaction temperature and forms a uniform and fluid material (mixed pyrolysis raw material), and then the high-temperature liquefied waste plastic mixed oil (mixed pyrolysis raw material) enters the pyrolysis reaction unit 5 (such as Figure 1 The mixed pyrolysis raw material is subjected to pyrolysis reaction in the pyrolysis reaction unit 5, and the gaseous product of the pyrolysis reaction enters the separation unit 6 (such as a fractionating tower) through the pipeline 11, and is separated in the fractionating tower to obtain gas (dry gas and liquefied gas), gasoline fraction, diesel fraction and wax oil fraction, which are respectively drawn out from pipelines 19, 12, 13 and 14, and the tail oil is drawn out from the bottom of the fractionating tower 6, wherein the diesel fraction is introduced into the heating unit 7 (heating furnace) through the pipeline 13, the wax oil fraction is introduced into the heating unit 7 through the pipeline 14, and the tail oil is introduced into the heating unit 7 through the pipeline 15 for heating (wherein, the wax oil fraction, the diesel fraction and the tail oil can be drawn out of the separation unit, Before entering the heating unit, they are first collected in a unified pipeline for mixing and then introduced into the heating unit); fresh pyrolysis raw materials (such as other process distillate oils) can be introduced into the bottom of the distillation tower 6 through pipeline 16 for preheating and then introduced into the heating unit 7 (heating furnace) for heating through pipeline 15, or fresh pyrolysis raw materials can be directly mixed with the wax oil fraction from pipeline 14 through pipeline 16 and then introduced into the heating unit 7 (heating furnace) for heating; the heated mixed material (including circulating oil and other fresh pyrolysis raw material oil) flowing out of the heating unit 7 enters the material mixing unit 3 as a mixed pyrolysis raw material.
[0070] The devices used in each unit in the present disclosure are all conventionally selected devices in the art.
[0071] The present invention is described in detail below with reference to examples, but the examples are not intended to limit the scope of application of the present invention.
[0072] Example 1
[0073] This example is used to illustrate the influence of different outlet temperatures of a twin-screw pump for dechlorination treatment on the dechlorination effect of waste plastics and the distribution results of pyrolysis products.
[0074] LDPE, HDPE, PS, PP and PVC are mixed in a mass percentage of 4:4:8:3:1, and the mixed plastic packaging material is crushed and dried. The chlorine content of the mixed plastic is 2.9% by weight as the chlorine-containing waste plastic raw material. A twin-screw pump is used as the equipment for the preliminary melting, liquefaction and dechlorination of the waste plastic, and the feed rate is about 100kg / h. Figure 1 The process shown specifically includes:
[0075] The chlorine-containing waste plastic raw material is introduced into a twin-screw pump, and heated, melted and dechlorinated under the shearing conditions of the twin-screw pump to obtain a dechlorinated waste plastic liquid phase material; the dechlorination reaction temperature is 285-330°C. The outlet temperature of the twin-screw pump is listed in Table 1 below, and liquefied dechlorinated waste plastics DCl-1-DCl-5 series are obtained. The properties of the obtained liquefied dechlorinated waste plastics are shown in Table 1.
[0076] The DCl-2 is heated to 430°C by a screw pump (i.e., the high-temperature liquefaction unit is introduced for further heating and viscosity reduction) to obtain high-temperature liquefied waste plastics, which are mixed with plastic pyrolysis oil heated to 520°C by a heating furnace (the material temperature of the mixture is 480°C), wherein the plastic pyrolysis oil refers to the wax oil fraction separated by the separation unit; the weight ratio of high-temperature liquefied waste plastics to plastic pyrolysis oil is 1:3; the mixture obtained by mixing high-temperature liquefied waste plastics and plastic pyrolysis oil enters the pyrolysis tower, and the product distribution obtained after the pyrolysis reaction products are separated by the separation unit is shown in Table 3, and the composition of dry gas and liquefied gas is shown in Table 4. The pyrolysis reaction conditions include: the pressure at the top of the pyrolysis tower is 0.1MPa, the pyrolysis reaction temperature is 480°C, and the time is 1h.
[0077] During the dechlorination process of the material, the hydrogen chloride gas is sucked out by vacuum equipment and introduced into the subsequent hydrogen chloride absorption unit for absorption. The vacuum degree in the twin-screw pump is 300 mmHg.
[0078] Example 2
[0079] The real waste plastic (PVC content is 9% by weight) is used as a twin-screw pump as a device for preliminary melting, liquefaction and dechlorination of waste plastics, with a feed rate of about 100 kg / h. Figure 1 The process shown and the method in Example 1 are different from Example 1 in that:
[0080] The outlet temperature of the twin-screw pump is 220°C; liquefied dechlorinated waste plastic DCl-6 is obtained, and the properties of the obtained liquefied dechlorinated waste plastic are shown in Table 2.
[0081] The DCl-6 was further heated to 475°C by a screw pump to obtain high-temperature liquefied waste plastics, which were mixed with plastic pyrolysis oil heated to 490°C by a heating furnace (the material temperature of the mixture was 460°C), wherein the plastic pyrolysis oil refers to the wax oil fraction separated by the separation unit; the ratio of high-temperature liquefied waste plastics to plastic pyrolysis oil was 1:1; the mixture of plastic and plastic pyrolysis oil entered the pyrolysis tower, and the distribution of pyrolysis reaction products was shown in Table 3, and the composition of dry gas and liquefied gas was shown in Table 4. The rest of the process was the same as in Example 1.
[0082] Example 3
[0083] The real waste plastic (PVC content is 8% by weight) is used as a twin-screw pump as a device for preliminary melting, liquefaction and dechlorination of the waste plastic, with a feed rate of about 100 kg / h. Figure 1 The process shown and the method in Example 1 are different from Example 1 in that:
[0084] The outlet temperature of the twin-screw pump is 320°C; liquefied dechlorinated waste plastic DCl-7 is obtained, and the properties of the obtained liquefied dechlorinated waste plastic are shown in Table 2.
[0085] The DCl-7 was further heated to 450°C by a screw pump to obtain high-temperature liquefied waste plastics, which were mixed with petroleum wax oil heated to 500°C by a heating furnace (the material temperature of the mixture was 465°C). The properties of the petroleum wax oil are shown in Table 5, and the ratio of plastic to petroleum wax oil is 1:1; the high-temperature liquefied waste plastics and petroleum wax oil mixture enters the pyrolysis tower, and the distribution of pyrolysis reaction products is shown in Table 3, and the composition of dry gas and liquefied gas is shown in Table 4. The rest of the process is the same as in Example 1.
[0086] Example 4
[0087] according to Figure 1 The process shown and the method in Example 3 are different from Example 3 in that:
[0088] All fractions above 350°C and part of fractions between 180 and 350°C in the pyrolysis product of DCl-7 are used as circulating oil (the weight ratio of fractions above 350°C to fractions between 180 and 350°C is 1:0.2), and are introduced into a heating furnace together with paraffin oil and heated to 500°C as high-temperature pyrolysis raw materials (the weight ratio of circulating oil to paraffin oil is 1:1); the ratio of high-temperature liquefied waste plastic to petroleum wax oil is 1:1; the mixture of plastic and petroleum wax oil (the material temperature of the mixture is 470°C) enters the pyrolysis tower, and the distribution of pyrolysis reaction products is shown in Table 3, and the composition of dry gas and liquefied gas is shown in Table 4. The rest of the process is the same as Example 3.
[0089] Comparative Example 1
[0090] according to Figure 1The process shown and the method in Example 3 are different from Example 3 in that:
[0091] After the DCl-7 was further heated to 450°C by a screw pump, it was directly introduced into the heating furnace and heated to 480°C, and then directly introduced into the pyrolysis tower for pyrolysis without mixing with circulating oil or petroleum wax oil. The results show that the furnace tubes of the heating furnace in this way are easily coked and blocked, and cannot be operated for a long period of time. Before the heating furnace coil is blocked, the distribution of pyrolysis reaction products is shown in Table 3, and the composition of dry gas and liquefied gas is shown in Table 4. The rest of the process is the same as Example 3.
[0092] Table 1
[0093] Sample name DCl-1 DCl-2 DCl-3 DCl-4 DCl-5 Outlet temperature 330 320 310 300 285 w(Cl) / (μg / g) 750 1630 1720 2900 6430 Dechlorination rate / % 97.41 94.38 94.07 90.00 77.83
[0094] According to the data in Table 1 above, when the temperature of the screw pump for dechlorination treatment is 300-375°C, the dechlorination rate is higher and can reach more than 90%.
[0095] Table 2
[0096] Example Example 2 Example 3 Sample name DCl-6 DCl-7 W(ash content) / % 23.05 0.517 W(C) / % 49.55 61 W(H) / % 7.22 8.3 W(Cl) / % 1.32 0.18 W(metal analysis) / (μg / g) Al 3010 1390 Ca 28710 220 Fe 8620 427 Mg 961 425 Na 1420 2460 Si 7090 207 Zn 304 538.2
[0097] According to the data in Table 2 above, by comparing the distribution of the liquefied dechlorinated waste plastic products in Example 2 and Example 3, it can be seen that the dechlorination temperature in Example 3 meets 300-375°C, and the chlorine content in the obtained liquefied dechlorinated waste plastic is lower.
[0098] Table 3 Distribution of pyrolysis products of waste plastics (dry basis)
[0099]
[0100] Table 4 Mass composition of dry gas and liquefied gas produced by pyrolysis of waste plastics
[0101]
[0102] According to the data in Tables 3 and 4 above, by comparing Example 3 with Comparative Example 1, the method and system for pyrolysis recovery of waste plastics provided by the present disclosure in Example 3 can reduce the yield of coke and dry gas; and the heating furnace tubes used in Comparative Example 1 are prone to coking and clogging, and cannot be operated for a long period of time.
[0103] Comparing Example 3 with Example 4, it can be seen that in Example 4, all fractions above 350°C and part of the fractions between 180 and 350°C in the pyrolysis product of DCl-7 are used as circulating oil together with petroleum wax oil as high-temperature pyrolysis raw materials and mixed with the dechlorinated waste plastic liquid phase material, and the coke yield is reduced.
[0104] In Example 1 of the present disclosure, the wax oil fraction obtained by the separation unit in the system is used as circulating oil to be mixed with high-temperature liquefied plastic (method 1), and in Example 3, petroleum wax oil is mixed with high-temperature liquefied plastic (method 2). The coke and dry gas yields in the product distribution obtained by the two methods are both low. Method 1 can be applied to places where petroleum wax oil cannot be obtained, such as garbage plants; Method 2 can be applied to places where petroleum wax oil resources are abundant. It shows that the present disclosure can be applied to different scenarios.
[0105] According to Tables 2 to 4, the real waste plastics used in Example 2 have a relatively high ash content. Although the coke content in the obtained product distribution reaches 30.03% by weight, the coke content produced by pyrolysis is about 7% by weight or less, and the content of liquefied gas and C5-180°C fraction in the pyrolysis product is also relatively high, indicating that the present disclosure can also achieve a better treatment effect on inferior waste plastic raw materials with a high ash content, and has a wide range of adaptability to waste plastic raw materials.
[0106] Table 5 Properties of petroleum wax oil
[0107] project Solvent wax oil <![CDATA[Density (20 °C) / (kg / m 3 )]]> 940.4 Residual carbon value / % 1.18 w(element) / % C 86.44 H 11.33 S 0.93 N 0.232 w(four-component composition) / % Saturated hydrocarbons 46.9 Aromatics 31.3 Gel 21.6 Asphaltene 0.2
[0108] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0109] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0110] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for pyrolysis recovery of waste plastics, characterized in that: The following steps are involved: S1. Allowing chlorine-containing waste plastics to enter a waste plastics preliminary melting, liquefaction and dechlorination unit (1) for hot melt dechlorination treatment to obtain a gas phase material containing hydrogen chloride and a dechlorinated waste plastics liquid phase material; wherein the waste plastics preliminary melting, liquefaction and dechlorination unit (1) comprises a first screw pump and a vacuum device connected to the first screw pump; the conditions of the hot melt dechlorination treatment include: an outlet temperature of 300-375°C; S2, allowing the dechlorinated waste plastic liquid phase material and the high-temperature pyrolysis raw material to enter the material mixing unit (3) respectively for mixing to obtain a mixed pyrolysis raw material; the temperature of the high-temperature pyrolysis raw material is 480° C. to 650° C.; S3, allowing the mixed pyrolysis raw material to enter the pyrolysis reaction unit (5) for pyrolysis to obtain pyrolysis gaseous products and coke; S4. The pyrolysis gaseous product enters a separation unit (6) for separation to obtain dry gas and liquefied gas, a gasoline fraction, a diesel fraction and a wax oil fraction.
2. The method according to claim 1, characterized in that The method further comprises: allowing the dechlorinated waste plastic liquid phase material obtained in step S1 to enter a high-temperature liquefaction unit (2) for heating treatment to obtain high-temperature liquefied waste plastic; and then allowing the high-temperature liquefied waste plastic to enter the material mixing unit (3); the heating treatment conditions of the high-temperature liquefaction unit (2) include: an outlet temperature of 400-500°C.
3. The method according to claim 2, characterized in that The high-temperature liquefaction unit (2) comprises a second screw pump, and the dechlorinated waste plastic liquid phase material is subjected to the heating treatment in the second screw pump; the conditions for the heating treatment include: an outlet temperature of 430-450°C.
4. The method according to claim 1, characterized in that: The method further comprises: allowing the pyrolysis raw material to enter a heating unit (7) for heating to obtain the high-temperature pyrolysis raw material; the temperature of the high-temperature pyrolysis raw material is 500° C. to 600° C.
5. The method according to claim 1, characterized in that In step S2, the weight ratio of the high-temperature pyrolysis raw material to the chlorine-containing waste plastic is 0.1-10:
1.
6. The method according to claim 5, characterized in that In step S2, the weight ratio of the high-temperature pyrolysis raw material to the chlorine-containing waste plastic is 0.3-5:
1.
7. The method according to claim 4, characterized in that The pyrolysis feedstock includes hydrocarbon oil; the hydrocarbon oil is selected from one or more of heavy crude oil, acidic crude oil, atmospheric residue oil, vacuum wax oil, coking wax oil, deasphalted oil, hydrocracking tail oil, coal tar, shale oil, tank bottom oil, and coal liquefaction residual oil.
8. The method according to claim 7, characterized in that The method further comprises: before entering the heating unit (7), allowing the hydrocarbon oil to enter the bottom of the tower of the separation unit (6) for preliminary preheating.
9. The method according to claim 4, characterized in that The separation unit (6) can also obtain tail oil after separation; the pyrolysis feedstock includes an external pyrolysis feedstock and optional circulating oil, and the circulating oil includes the wax oil fraction, the tail oil and the optional diesel fraction separated from the separation unit (6); the method further includes: Allowing the external pyrolysis raw material to enter the heating unit (7) for heating and then enter the material mixing unit (3) as the high-temperature pyrolysis raw material; or The circulating oil is allowed to enter the heating unit (7) for heating and then enters the material mixing unit (3) as the high-temperature pyrolysis raw material; or The circulating oil and the external pyrolysis raw material are allowed to enter the heating unit (7) together for heating, and the heated mixed material is then used as the high-temperature pyrolysis raw material and enters the material mixing unit (3).
10. The method according to claim 9, characterized in that The weight ratio of the circulating oil to the chlorine-containing waste plastic is 0.2-5.
0.
11. The method according to claim 10, characterized in that The weight ratio of the circulating oil to the chlorine-containing waste plastic is 0.2-2.
12. The method according to claim 1, characterized in that In step S1, the vacuum degree of the waste plastic preliminary melting, liquefaction and dechlorination unit (1) is 1-650 mmHg.
13. The method according to claim 12, characterized in that In step S1, the vacuum degree of the waste plastic preliminary melting, liquefaction and dechlorination unit (1) is 100-400 mmHg.
14. The method according to claim 1, characterized in that The chlorine-containing waste plastics include PVC and other plastics, wherein the other plastics are selected from one or more of LDPE, HDPE, PS, and PP; the content of the PVC is less than 10% by weight and not 0.
15. The method according to claim 14, characterized in that The ash content of the chlorine-containing waste plastic is less than 25% by weight.
16. The method according to claim 1, characterized in that The pyrolysis reaction unit (5) comprises a pyrolysis tower, the pressure at the top of the pyrolysis tower is 0.05-0.6 MPa, and the pyrolysis reaction temperature is 400-550°C.
17. The method according to claim 16, characterized in that The pyrolysis reaction unit (5) comprises a pyrolysis tower, the pressure at the top of the pyrolysis tower is 0.1-0.3 MPa, and the pyrolysis reaction temperature is 430-480°C.
18. The method according to claim 12, characterized in that The method further includes: The gaseous material containing hydrogen chloride obtained by the dechlorination unit (1) of the waste plastics is initially melted and liquefied, and enters the gaseous dechlorination unit (4) under the suction action of the vacuum device, and contacts with a hydrogen chloride absorbent to undergo hydrogen chloride absorption treatment; the gaseous phase after the hydrogen chloride absorption treatment and the dry gas separated by the separation unit (6) are introduced into a subsequent treatment device together; The hydrogen chloride absorbent is water or an alkali solution with a pH greater than 7, and the alkali solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution and ammonia water.
Citation Information
Patent Citations
Waste plastic continuous thermal cracking system and cracking method thereof
CN109401774A
Method and apparatus for co-converting waste plastic in delayed coker unit
CN112538363A
Delayed coking treatment method for waste plastics and treatment device thereof
CN101230284A
Method and device for preparing gasoline and diesel oil through cracking of waste plastics
CN107746722A
Oil refining process of waste plastic and equipment
CN1392224A