A catalyst for producing methanol from carbon dioxide hydrogenation and its preparation and application
The ZnO-ZrOx catalyst prepared by ball milling solves the problem of low catalytic activity of hydrogenation of carbon dioxide to methanol in the prior art, achieves high conversion and high selectivity, and is environmentally friendly in the process, reducing production costs.
Patent Information
- Application Number
- CN202310025447.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-09
AI Technical Summary
The existing carbon dioxide hydrogenation catalysts are low in catalytic activity under low temperature and low pressure conditions, insufficient conversion and selectivity, and complex preparation process.
The ZnO-ZrOx catalyst was prepared by ball milling method. By mixing Zn(NO3)2·6H2O, Zr(NO3)4·5H2O and citric acid, drying and calcining after ball milling, adjusting the molar ratio of Zn and Zr and the ball milling conditions to form uniform dispersion. The catalyst improves catalytic activity.
The CO2 conversion rate of more than 90% is maintained under the condition of 320-325°C, and the selectivity of methanol is maintained at more than 70%, which has high catalytic activity and high selectivity, and is environmentally friendly in the process, reducing production costs.
Smart Images

Figure CN116078370B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon dioxide hydrogenation utilization, in particular to a catalyst for preparing methanol by hydrogenation of carbon dioxide and the preparation and application thereof. Background Art
[0002] Methanol is a key raw material for industrial chemicals and can be further converted into polymer alternative liquid fuels. Renewable hydrogen energy can be used to reduce greenhouse gas carbon dioxide into high-value-added methanol.
[0003] High-efficiency catalysts have always been the key to hydrogenating carbon dioxide to methanol. The catalysts currently widely used in industry have the disadvantages of low conversion rate, selectivity and short life. For example, the modified ZnO catalyst can be found in the patent application document with publication number CN110052261A, entitled "A solid catalyst for selectively preparing methanol and carbon monoxide from carbon dioxide and its application", which discloses an In2O3 / ZnO-ZrO2 catalyst, and its preparation method is as follows: first, a mixture of any one or more of zirconium nitrate, zirconium chloride, zirconium oxychloride and any one or more of zinc nitrate, zinc chloride and zinc sulfate is reacted in an alkaline system composed of ammonium carbonate, sodium hydroxide, potassium hydroxide, etc. to generate ZnO-ZrO2, and then In2O3 is loaded, wherein the molar ratio of Zn to Zr is 1:6 to 6:1, and the loading amount of In is 1 mol% to 15 mol% based on the amount of ZnO-ZrO2 as 100%. The final In2O3 / ZnO-ZrO2 catalyst has a maximum CO2 conversion rate of 39.68% at 330°C and a CO2 conversion rate of 67.4% at 510°C. The catalytic activity of the catalyst increases with the increase of the catalytic temperature, but at the same time, the higher the reaction temperature, the lower the selectivity of methanol, and at a lower catalytic temperature, the catalytic activity is low and cannot meet the energy conservation and emission reduction requirements. Therefore, it is necessary to further study the ZnO catalyst used for catalytic hydrogenation of CO2 to produce methanol, to obtain ZnO-based catalysts with higher catalytic activity at lower catalytic temperatures, and to enrich the types of catalysts for catalytic hydrogenation of CO2 to produce methanol. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a catalyst for producing methanol by hydrogenation of carbon dioxide and its preparation and application, with the aim of solving the problems of complex catalyst preparation process, inability to catalyze the hydrogenation of carbon dioxide to produce methanol under low temperature and low pressure conditions, and poor conversion rate and selectivity of catalyzing carbon dioxide to produce methanol.
[0005] The technical solution adopted by the present invention is as follows:
[0006] The first aspect of the present application provides a method for preparing a catalyst for hydrogenating carbon dioxide to produce methanol. Zn(NO3)2·6H2O, Zr(NO3)4·5H2O and citric acid are weighed and mixed, and the mixture is ball-milled at a certain rotation speed. The reaction product after ball milling is dried and calcined to obtain a catalyst.
[0007] Further technical solutions are:
[0008] The molar ratio of Zn to (Zn+Zr) is 5% to 50%.
[0009] The molar ratio of Zn to (Zn+Zr) was 13%.
[0010] The molar ratio of (Zn+Zr) to citric acid is 1:(1.2-1.5).
[0011] The mass ratio of the grinding balls to the mixture used in ball milling is 4:1, and the rotation speed of the ball mill is 200-800 r / min.
[0012] The drying is carried out in an oven with a temperature of 105 to 120°C and a drying time of 12 to 20 hours.
[0013] The calcination is carried out in an air atmosphere at a temperature of 500 to 700° C. and a calcination time of 3 to 6 hours.
[0014] The second aspect of the present application provides a catalyst for producing methanol by hydrogenating carbon dioxide, which is prepared by the method described above.
[0015] The third aspect of the present application provides an application of the catalyst, wherein the catalyst is placed in a reactor, a hydrogen mixture is introduced, and the catalyst is reduced at 300-800°C for 2-6 hours; then a reaction mixture is introduced, and carbon dioxide is hydrogenated to produce methanol at 200-400°C and 2-8MPa.
[0016] Further technical solutions are:
[0017] The hydrogen mixed gas is a mixed gas of hydrogen and nitrogen, the reaction mixed gas is a mixed gas of carbon dioxide and hydrogen, the volume ratio of carbon dioxide to hydrogen is 1:(2-7), and the flow rate of the reaction mixed gas is 5-45 L / g cat / h.
[0018] The beneficial effects of the present invention are as follows:
[0019] Compared with other catalyst preparation methods, the catalyst preparation method of the present application adopts the ball milling method to not only make the components uniformly dispersed and stable in nature, but also assist in forming extremely abundant oxygen vacancies, which is conducive to providing more active sites and greatly improving the performance of the catalyst. The prepared catalyst is based on ZnZrOx It has high activity in the hydrogenation of carbon dioxide to methanol, can maintain a CO2 conversion rate of more than 90% at 320-325°C, and the methanol selectivity can be maintained at more than 70%. It has the characteristics of high catalytic activity and high methanol selectivity, and is more widely used.
[0020] The catalyst preparation method of the present application directly ball-mills the solid raw materials, and no waste liquid is generated during the preparation process. It is green and environmentally friendly, has a high raw material utilization rate, and greatly reduces environmental protection and production costs.
[0021] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The graph is a CO2 conversion rate graph of the catalysts prepared in Examples 1-4 of the present invention and the comparative example.
[0023] Figure 2 The methanol selectivity curves of the catalysts prepared in Examples 1-4 of the present invention and the comparative example are shown.
[0024] Figure 3 The X-ray powder diffraction patterns of the catalysts prepared in Example 2 of the present invention and the comparative example.
[0025] Figure 4 O of the catalyst prepared in Example 2 of the present invention and the comparative example 1s XPS analysis chart. DETAILED DESCRIPTION
[0026] The specific implementation of the present invention is described below with reference to the accompanying drawings.
[0027] The present application provides a method for preparing a catalyst for producing methanol by hydrogenating carbon dioxide. Zn(NO3)2·6H2O, Zr(NO3)4·5H2O and citric acid are weighed and mixed, and the mixture is ball-milled at a certain rotation speed. The reaction product after ball milling is dried and calcined to obtain a catalyst.
[0028] The molar ratio of Zn to (Zn+Zr) is 5% to 50%.
[0029] The molar ratio of Zn to (Zn+Zr) is 13%.
[0030] Among them, the molar ratio of (Zn+Zr) to citric acid is 1:(1.2-1.5).
[0031] The mass ratio of the grinding balls to the mixture used in ball milling is 4:1, and the rotation speed of the ball mill is 200-800 r / min.
[0032] The drying is carried out in an oven, the oven temperature is 105-120° C., and the drying time is 12-20 hours.
[0033] The calcination is carried out in an air atmosphere, the calcination temperature is 500-700° C., and the calcination time is 3-6 hours.
[0034] The catalyst preparation method of the present application reasonably sets different rotation speeds in the ball milling method and the molar ratio of each component in the catalyst. The prepared catalyst can be used in the carbon dioxide hydrogenation to methanol reaction, which can effectively improve the problems of low carbon dioxide conversion rate and low product selectivity.
[0035] The following examples 1-4 further illustrate the preparation method of the catalyst for hydrogenating carbon dioxide to methanol of the present application.
[0036] Example 1
[0037] Weigh zirconium nitrate and zinc nitrate according to the molar ratio of Zn / (Zn+Zr) of 13%, weigh citric acid so that the molar ratio of (Zn+Zr): citric acid is 1:1.2, weigh grinding balls so that the mass ratio of grinding balls to total feed is 4:1, put the grinding balls and total feed into the jar of the ball mill, set the ball mill speed to 200r / min, and make the feed fully react at 200r / min for 2h. Take out the sample and dry it at 110℃ for 20h, and then calcine it at 600℃ for 4h to obtain the catalyst, which is recorded as catalyst A.
[0038] Example 2
[0039] The same method as in Example 1 was adopted, with other conditions being the same as in Example 1, except that the rotation speed of the ball mill was 300 r / min. The obtained catalyst was recorded as Catalyst B.
[0040] Example 3
[0041] The same method as in Example 1 was adopted, with other conditions being the same as in Example 1, except that the rotation speed of the ball mill was 400 r / min. The obtained catalyst was recorded as Catalyst C.
[0042] Example 4
[0043] The same method as in Example 1 was adopted, with other conditions being the same as in Example 1, except that the rotation speed of the ball mill was 500 r / min. The obtained catalyst was recorded as Catalyst D.
[0044] The comparison example for the above embodiment is as follows:
[0045] Comparative Example
[0046] The ZnO-ZrOx catalyst was prepared by co-precipitation method, and the specific steps are as follows:
[0047] Zirconium nitrate and zinc nitrate were weighed according to a molar ratio of Zn / (Zn+Zr) of 13%, dissolved in 100 mL of deionized water, and 100 mL of 0.2 M ammonium carbonate solution was added dropwise at a rate of 3 mL / min in a 70°C water bath. After the addition was complete, the mixture was reacted for 2 h, filtered, dried at 110°C for 20 h, and then calcined at 600°C for 4 h. The resulting catalyst was recorded as Catalyst E.
[0048] The catalysts obtained in Examples 1-4 and the comparative example were applied to the reaction of hydrogenating carbon dioxide to produce methanol, and the specific steps were as follows:
[0049] A vertical tubular heating furnace reactor with an inner diameter of 10 mm and a temperature control system was used. 0.1 mg of catalyst was loaded into the reactor, and a mixture of hydrogen and nitrogen was introduced. The catalyst was reduced at 300-800°C for 2-6 hours. Then the reaction mixture was introduced, and the carbon dioxide hydrogenation to methanol reaction was carried out at 200-400°C and 2-8MPa.
[0050] The total nitrogen intake was 40 mL / min, the volume concentration of the reaction mixture CO2 was 24%, the volume concentration of H2 was 72%, and each reaction temperature was continuously tested for 2 h, with a test temperature interval of 40 °C. The activity results of the catalyst were expressed in terms of CO2 conversion and methanol selectivity, and the CO2 concentration and methanol concentration were detected using online gas chromatography. The test results are shown in Table 1.
[0051] Table 1 Activity of the catalysts obtained in Examples 1-4 and Comparative Examples
[0052] catalyst <![CDATA[CO2 conversion rate / %]]> <![CDATA[CH3OH selectivity / %]]> A 12.1 89.5 B 15.3 91.8 C 17.5 90.5 D 19.9 92.3 E 10.2 87.6
[0053] As shown in Table 1, the metal catalysts prepared by the preparation method of the present application have a high CO2 conversion rate and a high methanol selectivity. Among them, the catalytic performance of the catalyst D prepared in Example 4 is the best, which is significantly better than that of the comparative example catalyst E, indicating that the performance of the catalyst prepared by the ball milling method is better than that of the ZnO-ZrO prepared by the coprecipitation method in terms of CO2 conversion rate and methanol selectivity. x catalyst.
[0054] Depend on Figure 1 and Figure 2 It can be seen that the catalyst prepared by the present invention has a higher CO2 conversion rate and a higher methanol selectivity than the catalyst prepared by the coprecipitation method. Among them, the catalyst D prepared in Example 4 has the best catalytic performance. The CO2 conversion rate can reach 19.9% at 320°C, and the methanol selectivity reaches 92.3%. Figure 1It can be seen that with the increase of reaction temperature, the conversion rate gradually increases, while the methanol selectivity decreases due to thermodynamic limitations. Therefore, the data in Table 1 are selected from the results at the most preferred temperature of each catalyst.
[0055] Figure 3 The X-ray powder diffraction patterns of the catalysts prepared in Example 2 and the comparative example. The center of the diffraction peak observed at 30.26° in the figure corresponds to the (011) plane, which is a typical t-ZrO2 diffraction peak. The center of the diffraction peak observed at 35.25° in the figure corresponds to the (111) plane, which is a typical m-ZrO2 diffraction peak. It can be seen that in the prepared catalyst, the more obvious crystal form is the t-ZrO2 diffraction peak, and the grains thereof are analyzed, and the grains of the ball milling method (9.1nm) are smaller than the grains of the catalyst prepared by the co-precipitation method (15.4nm).
[0056] Figure 4 O of the catalyst prepared in Example 2 and the comparative example 1s XPS analysis diagram of O Ⅰ (lattice oxygen), 531.7 eV corresponds to O Ⅱ (ortho-defective oxygen), 532.7 eV corresponds to O Ⅲ (Adsorbed oxygen). O of the catalyst prepared by ball milling Ⅲ The content ratio is less than that of co-precipitation method, while O Ⅰ The increase in content indicates that O Ⅰ (Lattice oxygen) contributes to the reaction activity.
[0057] Those skilled in the art can understand that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for producing methanol by hydrogenation of carbon dioxide, characterized in that: Weigh Zn(NO3)2·6H2O, Zr(NO3)4·5H2O and citric acid and mix them, ball-mill the mixture at a certain speed, and dry and calcine the reaction product after ball milling to obtain a catalyst; The molar ratio of Zn to (Zn + Zr) is 13%; The molar ratio of (Zn+Zr) to citric acid is 1:(1.2-1.5); The mass ratio of the grinding balls to the mixture used in ball milling was 4:1, and the rotation speed of the ball mill was 500 r / min.
2. The method for preparing a catalyst for producing methanol by hydrogenation of carbon dioxide according to claim 1, characterized in that: The drying is carried out in an oven with a temperature of 105 to 120°C and a drying time of 12 to 20 hours.
3. The method for preparing a catalyst for producing methanol by hydrogenation of carbon dioxide according to claim 1, characterized in that: The calcination is carried out in an air atmosphere at a temperature of 500 to 700° C. and a calcination time of 3 to 6 hours.
4. A catalyst for producing methanol by hydrogenating carbon dioxide, characterized in that: The method is prepared by the method according to any one of claims 1 to 3.
5. Use of the catalyst as claimed in claim 4, characterized in that: The catalyst is placed in a reactor, a hydrogen mixed gas is introduced, and the catalyst is reduced at 300-800° C. for 2-6 hours; then a reaction mixed gas is introduced, and a carbon dioxide hydrogenation to methanol reaction is carried out at 200-400° C. and 2-8 MPa.
6. Use of the catalyst according to claim 5, characterized in that: The hydrogen mixed gas is a mixed gas of hydrogen and nitrogen, the reaction mixed gas is a mixed gas of carbon dioxide and hydrogen, the volume ratio of carbon dioxide to hydrogen is 1: (2-7), and the flow rate of the reaction mixed gas is 5-45 L / g cat / h.