A catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine and its application

Through the preparation of tin-antimony mesoporous carbon catalyst, the problems of low efficiency and unenvironmental protection of existing catalysts in catalytic ammonia oxidation reaction are solved, and efficient and environmentally friendly preparation of 2-cyanopyridine with long life and low cost Advantages.

CN116078371BActive Publication Date: 2024-12-03NANTONG LIYANG CHEM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211728201.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-12-03
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The existing catalysts have low catalytic efficiency, many by-products, high cost and unenvironmental protection in catalytic ammonia oxidation reactions, resulting in insufficient yield and selectivity of 2-cyanopyridine, which is difficult to meet the needs of industrial production.

Method used

Using tin-antimony mesoporous carbon catalyst, the specific preparation method and process conditions include using mesoporous carbon as a support, loading tin dioxide and antimony trioxide, and performing acid leaching and calcining procedures to improve the specific surface area of ​​the catalyst. and porosity, thereby improving catalytic activity and service life.

Benefits of technology

It achieves high conversion and high selectivity preparation of 2-cyanopyridine, with a long service life, simple process, low cost, and meets green and environmental protection requirements, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the field of catalytic synthesis technology, and specifically relates to a catalyst for catalyzing ammoxidation to prepare 2-cyanopyridine and its application. The present invention selects mesoporous carbon as a carrier, loads a specific proportion of tin dioxide and antimony trioxide, and obtains a catalyst for ammoxidation reaction with high catalytic activity. The tin-antimony mesoporous carbon catalyst of the present invention has high specific surface area and porosity, high catalytic activity and efficiency, can be recycled for multiple uses, has a long life, only requires two active metal raw materials to maintain excellent catalytic performance, and the preparation process is simple, which reduces costs. The present invention uses waste straw to prepare mesoporous carbon, which is green and environmentally friendly, and the mesoporous carbon of the present invention has high porosity and strong adsorption capacity for active metals. When the tin-antimony mesoporous carbon catalyst of the present invention catalyzes ammoxidation to prepare 2-cyanopyridine, the raw material conversion rate is>99.9%, the 2-cyanopyridine selectivity is>90%, and the yield is ≥90%, which has great industrial value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalytic synthesis, in particular to the field under IPC classification number B01J 27 / 19, and more specifically to a catalyst for preparing 2-cyanopyridine by catalytic ammoxidation reaction and application thereof. Background Art

[0002] 2-cyanopyridine is an important fine organic synthesis intermediate, which is widely used in the production of fine organic chemicals such as various medicines, pesticides and dyes, such as the synthesis of agricultural herbicides 4-amino-3,5,6-trichloropyridine-2-carboxylic acid (picloram) and Xa factor inhibitor betrixaban. In the preparation process of 2-cyanopyridine, the 2-methylpyridine catalytic ammoxidation method has been widely used in actual production due to the characteristics of sufficient raw material sources, no highly toxic cyanide, and relatively low product preparation cost. However, the ammoxidation reaction is a complicated process. In addition to the main reaction, there are many side reactions, which greatly reduce the yield of dicyanopyridine. Therefore, it is the key to the ammoxidation synthesis technology of 2-cyanopyridine to study a new catalyst with good selectivity and high conversion rate, optimize process conditions, and reduce production costs.

[0003] At present, most catalysts for catalytic ammoxidation reaction to synthesize cyanopyridine are prepared by impregnation method, also known as equal volume impregnation method, that is, adding a solution sufficient to fill the pore volume of the carrier particles or slightly less, and supporting it on the porous carrier. For powdered carriers, the volume of the impregnation liquid needs to be slightly larger than the pore volume (called wet impregnation), unless the catalyst precursor can be strongly adsorbed on the carrier. Especially during the drying period, it is important to continuously stir the slurry to ensure that the catalyst precursor is evenly distributed on the carrier. The commonly used carrier in the current prior art is titanium dioxide.

[0004] The main components and contents of the ammoxidation catalyst used in the current process are V:Mo:Cr:P:TiO2=10-30%:0-1%:0-1%:0-1%:70-90%. In production, it can only make the conversion rate of 2-methylpyridine>98%, the selectivity of the product 2-cyanopyridine>88%, and the yield ≥82%; the catalytic active part in the catalyst is a variety of metal compounds, the process is not only complicated, but also has low catalytic efficiency and many by-products. Prior art CN103467370B discloses a method for synthesizing cyanopyridine, the catalyst used is a vanadium titanium catalyst, which needs to be prepared with a variety of metal compounds, which is costly and not environmentally friendly, and the efficiency of catalyzing the ammoxidation of 2-methylpyridine to prepare 2-cyanopyridine is not high, and the yield is only about 70-80%. Summary of the invention

[0005] In view of the defects of the prior art, the object of the present invention is to provide a catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine, which has high activity, high raw material conversion rate and product selectivity, high yield, long service life, simple production process and is green and environmentally friendly.

[0006] On the other hand, the present invention also aims to provide an application of the above-mentioned catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A catalyst for catalyzing an ammoxidation reaction to prepare 2-cyanopyridine, characterized in that the catalyst is a tin-antimony mesoporous carbon catalyst prepared by the following method:

[0009] Mesoporous carbon is added to a mixed solution of tin dioxide and antimony trioxide, stirred and mixed, dried, calcined, acid-leached, washed with water, filtered and dried to obtain a tin-antimony mesoporous carbon catalyst.

[0010] Preferably, in the mixed solution of tin dioxide and antimony trioxide, the concentration of tin dioxide is 0.04-0.07 g / mL, and the concentration of antimony trioxide is 0.02-0.05 g / mL.

[0011] Preferably, the stirring time for stirring and mixing is 1 to 3 hours;

[0012] Preferably, the drying operation is stirring at 70-100°C until dry, and then drying at 110-130°C;

[0013] Preferably, the temperature raising procedure of the calcination is to raise the temperature to 800-1000° C. at a rate of 2-5° C. / min, and then keep the temperature for 2-5 hours.

[0014] Preferably, the acid used in the acid leaching treatment is dilute hydrochloric acid, dilute sulfuric acid or dilute nitric acid; more preferably, the mass concentration of the dilute hydrochloric acid is 5%.

[0015] Preferably, the acid leaching treatment is performed by soaking and shaking the calcined product in acid to remove impurities.

[0016] Preferably, the mass fraction of tin element in the catalyst is 20-30%, and the mass fraction of antimony element is 25-35%.

[0017] Preferably, the specific surface area of ​​the catalyst is 850 to 1200 m 2 / g.

[0018] Preferably, the pore size of the catalyst is 5.5 to 10.8 nm.

[0019] The present invention selects mesoporous carbon as a carrier, loads tin dioxide and antimony trioxide in a specific ratio, and obtains an ammoxidation catalyst with high catalytic activity. The present invention creatively discovers the excellent catalytic activity of tin-antimony active bimetal for ammoxidation reaction, significantly improving the conversion rate of 2-methylpyridine raw material and the selectivity of 2-cyanopyridine product. The inventors also found that increasing the loading amount of tin-antimony in the catalyst within a certain range is conducive to improving the product yield, especially when the tin loading amount is 25% and the antimony loading amount is 30%, the yield of 2-cyanopyridine prepared by the ammoxidation reaction catalyzed by it can reach 90.8%; but when the tin loading amount exceeds 30% and the antimony loading amount exceeds 35%, the yield of the product decreases instead. The inventors speculate that it may be because the excessive loading amount causes the specific surface area of ​​the catalyst to decrease, and the pore size to increase, resulting in a smaller effective surface area, and the catalytic efficiency is correspondingly reduced. The invention increases the effective surface area of ​​the catalyst, thereby improving the catalytic activity and service life of the catalyst by specifically limiting the calcination procedure and the acid leaching treatment method in the catalyst preparation process and adjusting the loading amount of the active metal.

[0020] Preferably, the mesoporous carbon is prepared by the following steps:

[0021] S1: mixing straw with inorganic acid for reaction, filtering, adding alkaline solution for activation, and drying to obtain a mesoporous carbon precursor;

[0022] S2: calcining the mesoporous carbon precursor under the protection of an inert gas, soaking it with a strong acid after calcination, washing it with water after removing impurities, and drying it to obtain the mesoporous carbon.

[0023] Preferably, the straw is chopped waste straw;

[0024] Preferably, the inorganic acid is dilute hydrochloric acid, dilute sulfuric acid or dilute nitric acid;

[0025] Preferably, the reaction time is 10 to 15 hours;

[0026] Preferably, the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution;

[0027] Preferably, the drying operation in step S1 is stirring at 70-100°C until dry, and then drying at 110-130°C;

[0028] Preferably, the inert gas is nitrogen or argon;

[0029] Preferably, the temperature raising procedure of the calcination in step S2 is to raise the temperature to 500-700° C. at a rate of 1-3° C. / min, and then keep the temperature for 2-5 hours.

[0030] Preferably, the strong acid is hydrofluoric acid, hypochlorous acid, hydrochloric acid or sulfuric acid; further preferably, the strong acid is 10 wt % hydrofluoric acid.

[0031] The present invention selects discarded straw as the material for preparing mesoporous carbon, realizes waste utilization, has sufficient raw materials, can be mass-produced, not only reduces costs, but also meets the requirements of green chemical industry. In addition, the present invention first uses acid and alkali to pre-carbonize the straw, which can cause the fiber of the straw to break first, shorten the time required for calcination and carbonization, and reduce the temperature required for calcination. The inventors also found that the adsorption of active metals by mesoporous carbon without impurities is greatly different, and the concentration and type of acid in the preparation process, the calcination temperature, and the drying operation will affect the removal of impurities in the mesoporous carbon. The present invention specifically selects dilute sulfuric acid to pre-carbonize the straw, and soaks it with 10wt% hydrofluoric acid after calcination. The obtained mesoporous carbon has a higher porosity and specific surface area, thereby allowing the loading amount of active metals to be adjusted in a larger range. In addition, considering that direct high-temperature drying of mesoporous carbon powder is prone to agglomeration, the present invention also stirs it to dryness at a lower temperature before drying, and this operation is also conducive to obtaining a higher specific surface area.

[0032] Another aspect of the present invention provides an application of the above catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine, which is applied to catalyzing ammoxidation of 2-methylpyridine to prepare 2-cyanopyridine.

[0033] Preferably, the step of preparing 2-cyanopyridine by ammoxidation of 2-methylpyridine comprises: loading the above-mentioned catalyst into a tubular fixed bed reactor, adding 2-methylpyridine and ammonia water, introducing oxygen-containing gas and ammonia gas, reacting to obtain reaction gas, and condensing, stratifying and distilling the reaction gas to obtain the finished product 2-cyanopyridine.

[0034] Preferably, the molar ratio of the oxygen-containing gas, 2-methylpyridine, ammonia gas and ammonia water is 200-300:1-2:40-60:0.5-2; more preferably, it is 245:1.1:54:1;

[0035] Preferably, the oxygen-containing gas is air.

[0036] Preferably, the filling amount of the catalyst is 800-1200 mL; more preferably, it is 1000 mL.

[0037] Preferably, after the catalyst is loaded into the tubular fixed bed reactor, the temperature is raised to 350-400° C.;

[0038] Preferably, the preheating temperature of the 2-methylpyridine, ammonia water, oxygen-containing gas and ammonia gas before entering the reactor is 220-230°C;

[0039] Preferably, the specific operation of the layering is to layer the crude 2-cyanopyridine in the lower layer in the layering kettle, and control the residence time of the crude 2-cyanopyridine in the layering kettle to be 20 to 30 minutes.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. The tin-antimony mesoporous carbon catalyst of the present invention has a high specific surface area and porosity, high catalytic activity and efficiency, can be recycled for multiple times, and has a long service life;

[0042] 2. The tin-antimony mesoporous carbon catalyst of the present invention requires only two active metal raw materials, has a simple preparation process, is low in cost, and can still maintain excellent catalytic performance;

[0043] 3. The mesoporous carbon used in the tin-antimony mesoporous carbon catalyst of the present invention is prepared from waste straw as raw material, which is waste utilization, green and environmentally friendly, and suitable for industrial production;

[0044] 4. The mesoporous carbon prepared by the method of the present invention has high porosity and strong adsorption capacity for active metals. The raw material utilization rate is high when preparing tin-antimony mesoporous carbon catalysts, and a higher content of active metals can be loaded, which is beneficial to reducing the amount of catalyst used;

[0045] 5. When the tin-antimony mesoporous carbon catalyst of the present invention catalyzes ammoxidation to prepare 2-cyanopyridine, the conversion rate of the raw material 2-methylpyridine is >99.9%, the selectivity of the product 2-cyanopyridine is >90%, and the yield is ≥90%, which can effectively save costs and has great industrial value. DETAILED DESCRIPTION

[0046] Example 1

[0047] This embodiment provides a catalyst for catalyzing an ammoxidation reaction to prepare 2-cyanopyridine, wherein the catalyst is a tin-antimony mesoporous carbon catalyst, which is prepared by the following method:

[0048] A mixed solution of tin dioxide and antimony trioxide was prepared with 200 ml of deionized water, 8.4 g of tin dioxide and 5 g of antimony trioxide; 10.0 g of mesoporous carbon was added to the mixed solution of tin dioxide and antimony trioxide, stirred and mixed evenly for 2 hours, and then stirred in a water bath at 85°C until dry. Dry at 120°C overnight, and in a calcining furnace, under nitrogen protection, heat to 900°C at a rate of 3°C / min, and keep warm for 2 hours. After calcination, soak and shake overnight with 5% hydrochloric acid to remove impurities, and finally wash with deionized water until the water is neutral, and dry at 120°C for 2 hours to obtain a tin-antimony mesoporous carbon catalyst.

[0049] The mesoporous carbon is prepared by the following steps:

[0050] S1: 10 g of chopped waste straw and 200 mL of dilute sulfuric acid were placed in a reactor, reacted at 150°C for 12 h, filtered, activated by adding 30 mL of 0.5 M NaOH solution, stirred at 85°C until dry, and dried at 120°C overnight to obtain a mesoporous carbon precursor.

[0051] S2: In a calcination furnace, under nitrogen protection, the temperature was raised to 600°C at a rate of 2°C / min, kept warm for 3 hours, calcined and carbonized, and after calcination, soaked and shaken in 200mL 10wt% hydrofluoric acid overnight to remove impurities, and finally washed with deionized water until the washing water was neutral, and dried at 120°C for 2 hours to obtain mesoporous carbon.

[0052] The tin-antimony mesoporous carbon catalyst (20Sn-25Sb / BC) prepared in this example has a tin loading of 20%, an antimony loading of 25%, and a specific surface area of ​​1010 m 2 / g, pore size 7.4nm.

[0053] On the other hand, the present embodiment provides an application of the above-mentioned catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine, which is applied to catalyzing ammoxidation of 2-methylpyridine to prepare 2-cyanopyridine. The specific steps are: filling 1000 mL of the tin-antimony mesoporous carbon catalyst (20Sn-25Sb / BC) of the present embodiment in a tubular fixed bed microreactor, heating the reactor filled with the catalyst to 350° C., using industrial 2-methylpyridine and ammonia water as raw materials, introducing air and ammonia gas for reaction, and controlling The preheating temperature of 2-picoline, ammonia, oxygen and ammonia before entering the reactor is 230°C; the molar ratio of air, 2-picoline, ammonia and ammonia is 245:1.1:54:1, the reaction time is about 2 seconds, and the reaction gas is obtained. The reaction gas is condensed, and the condensate is layered in a layered kettle. The residence time of the lower layer of 2-cyanopyridine in the layered kettle is controlled to be 30 minutes, and the lower layer of 2-cyanopyridine is continuously pumped into the distillation kettle, and the kettle temperature is 140°C to obtain the 2-cyanopyridine finished product. The raw material conversion rate and product yield are determined by liquid chromatography. In this embodiment, the 2-picoline conversion rate is 99.9%, and the 2-cyanopyridine yield is 88.6%.

[0054] Example 2

[0055] This embodiment provides a catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine and its application. The specific implementation method is the same as that of Example 1, except that: the mixed solution of tin dioxide and antimony trioxide is prepared from 200 ml of deionized water, 10.4 g of tin dioxide and 5 g of antimony trioxide.

[0056] The tin-antimony mesoporous carbon catalyst (25Sn-25Sb / BC) prepared in this embodiment has a tin loading of 25%, an antimony loading of 25%, and a specific surface area of ​​1021m 2 / g, pore size 6.8nm.

[0057] In this example, the conversion rate of 2-methylpyridine is 99.9%, and the yield of 2-cyanopyridine is 89.2%.

[0058] Example 3

[0059] This embodiment provides a catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine and its application. The specific implementation method is the same as that of Example 1, except that: the mixed solution of tin dioxide and antimony trioxide is prepared from 200 ml of deionized water, 8.4 g of tin dioxide and 8 g of antimony trioxide.

[0060] The tin-antimony mesoporous carbon catalyst (20Sn-30Sb / BC) prepared in this embodiment has a tin loading of 20%, an antimony loading of 30%, and a specific surface area of ​​1015m 2 / g, pore size 6.5nm.

[0061] In this example, the conversion rate of 2-methylpyridine is 99.9%, and the yield of 2-cyanopyridine is 89.4%.

[0062] Example 4

[0063] This embodiment provides a catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine and its application. The specific implementation method is the same as that of Example 1, except that: the mixed solution of tin dioxide and antimony trioxide is prepared from 200 ml of deionized water, 10.4 g of tin dioxide and 8 g of antimony trioxide.

[0064] The tin-antimony mesoporous carbon catalyst (25Sn-30Sb / BC) prepared in this example has a tin loading of 25%, an antimony loading of 30%, and a specific surface area of ​​1108 m 2 / g, pore size 5.9nm.

[0065] In this example, the conversion rate of 2-methylpyridine is 99.9%, and the yield of 2-cyanopyridine is 90.8%.

[0066] Example 5

[0067] This embodiment provides a catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine and its application. The specific implementation method is the same as that of Example 1, except that: the mixed solution of tin dioxide and antimony trioxide is prepared from 200 ml of deionized water, 12.5 g of tin dioxide and 9.4 g of antimony trioxide.

[0068] The tin-antimony mesoporous carbon catalyst (30Sn-35Sb / BC) prepared in this example has a tin loading of 30%, an antimony loading of 35%, and a specific surface area of ​​997 m 2 / g, pore size 7.8nm.

[0069] In this example, the conversion rate of 2-methylpyridine is 99.9%, and the yield of 2-cyanopyridine is 86.7%.

Claims

1. A catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine, characterized in that: The catalyst is a tin-antimony mesoporous carbon catalyst, which is prepared by the following method: Mesoporous carbon is added to a mixed solution of tin dioxide and antimony trioxide, stirred and mixed, dried, calcined, acid-leached, washed, filtered and dried to obtain a tin-antimony mesoporous carbon catalyst; The concentration of tin dioxide in the mixed solution of tin dioxide and antimony trioxide is 0.04-0.07 g / mL, and the concentration of antimony trioxide is 0.02-0.05 g / mL; the mass fraction of tin element in the catalyst is 20-30%, and the mass fraction of antimony element is 25-35%; The calcination temperature program is to increase the temperature to 800-1000°C at a rate of 2-5°C / min, and then keep the temperature for 2-5h; The specific surface area of ​​the catalyst is 850-1200 m 2 / g; The pore size of the catalyst is 5.5-10.8 nm; The mesoporous carbon is prepared by the following steps: S1: mixing straw with inorganic acid for reaction, filtering, adding alkaline solution for activation, and drying to obtain a mesoporous carbon precursor; S2: calcining the mesoporous carbon precursor under the protection of an inert gas, soaking it with a strong acid after calcination, washing it with water after removing impurities, and drying it to obtain mesoporous carbon; The temperature raising procedure of the calcination in the step S2 is to raise the temperature to 500-700° C. at a rate of 1-3° C. / min and then keep the temperature for 2-5 hours.

2. Use of the catalyst for preparing 2-cyanopyridine by catalytic ammoxidation reaction according to claim 1, characterized in that: It is used to catalyze the ammoxidation of 2-methylpyridine to prepare 2-cyanopyridine.

3. The use of the catalyst for catalyzing ammoxidation reaction to prepare 2-cyanopyridine according to claim 2, characterized in that: The step of preparing 2-cyanopyridine by ammoxidation of 2-methylpyridine comprises: filling the catalyst according to claim 1 in a tubular fixed bed reactor, adding 2-methylpyridine and ammonia water, introducing oxygen-containing gas and ammonia gas, reacting to obtain reaction gas, and condensing, stratifying and distilling the reaction gas to obtain the finished product 2-cyanopyridine.