A capsule asphalt modifier and preparation method thereof

Using supercritical fluids to prepare porous capsule shells to encapsulate liquid modifiers solves the problems of loss and poor dispersion of direct-thrown asphalt modifiers in high-temperature processing, and achieves uniform dispersion and efficient modification of modifiers in asphalt. safety, simplifying the process and reducing energy consumption.

CN116082850BActive Publication Date: 2024-10-22NANJING XUZHI MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211102051.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-10-22
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

Existing direct-throw asphalt modifiers have problems with loss and poor dispersion during high-temperature processing, making it difficult to meet the specifications of modified asphalt, and have poor compatibility and instant solubility in the dry modification process.

Method used

The porous polymer capsule shell is prepared through a supercritical fluid pore-forming process, and the liquid modifier is encapsulated to form a solid-liquid integrated capsule asphalt modifier. Capillary action is used to achieve uniform dispersion of the modifier in the asphalt.

Benefits of technology

It avoids high-temperature processing losses, achieves uniform dispersion and efficient modification of modifiers, reduces energy consumption, simplifies the process flow, and improves engineering efficiency and modification effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116082850B_ABST
    Figure CN116082850B_ABST
Patent Text Reader

Abstract

The present invention discloses a direct-cast capsule asphalt modifier and a preparation method thereof. The capsule asphalt modifier of the present invention comprises 10-50 parts by mass of a polymer capsule shell and 30-90 parts by mass of a liquid modifier core. The direct-cast capsule asphalt modifier of the present invention uses supercritical pore-making technology to prepare a polymer modifier into a shell with a microporous structure, and then encapsulates the liquid modifier in the shell through capillary action, thereby solving the problems of difficult storage and transportation of liquid modifiers and large investment in equipment for on-site use. The direct-cast capsule asphalt modifier can be directly put into an asphalt tank or asphalt mixture on site, and can significantly improve the low-temperature crack resistance, room-temperature fatigue resistance, and high-temperature flow resistance of asphalt through simple stirring, thereby enhancing the comprehensive road performance of the asphalt binder. In addition, the preparation process of the capsule asphalt modifier of the present invention is simple and convenient for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of road and bridge materials, and in particular to an asphalt modifier and a preparation method thereof. Background Art

[0002] At present, more than 95% of modified asphalt is still produced by wet modification in factories. It is necessary to add solid polymers and liquid rubber oil and other modifiers into large colloid mills, and obtain modified asphalt products through high-speed shearing and dispersion, and then store them in factory asphalt tanks. When used on the construction site, it is transferred to the on-site asphalt tank by a special asphalt transport vehicle. This wet modified asphalt process is cumbersome, requires large equipment investment, and consumes high energy, which does not meet the current green and low-carbon development goals. The direct-injection asphalt modifier gets rid of the high energy consumption and other problems in the production process of wet modified asphalt, realizes on-site modification, greatly improves engineering efficiency, reduces engineering expenses, and reduces carbon dioxide emissions.

[0003] At present, direct-cast modifiers are prepared by melt blending polymers such as SBS and additives. However, there are two problems in the production of asphalt modifiers by melt blending process. First, the content of liquid modifier components in the modifier cannot be too high, otherwise it cannot be formed. In addition, liquid modifiers will be lost during high-temperature processing, resulting in failure of the final ratio. Therefore, it is often difficult to meet the modified asphalt index in practical applications, and it is also necessary to add additional additives such as rubber oil or select a specific grade of matrix asphalt for modification. Secondly, the asphalt modifier prepared by melt blending process has poor compatibility and solubility in asphalt, and still requires high-speed shearing to achieve dispersion. At present, although there is a patent (CN 114163830 A) that locally swells polymers such as SBS by adding a large amount of plasticizers, the purpose of rapid melting is achieved at high temperature. However, the polarity of polymer modifiers and asphalt phases is quite different. Although the swollen polymer particles can melt quickly at high temperatures, it is difficult to achieve uniform dispersion of the modifier in the asphalt phase by simple stirring, and the modifier is still distributed in the asphalt phase as a large block melt. Therefore, the current dry-process asphalt modification process using direct-injection asphalt modifiers cannot completely replace the wet-process modification process. Therefore, there is an urgent need to prepare a direct-injection asphalt modifier with a modification effect comparable to that of the wet-process. Summary of the invention

[0004] The technical problem to be solved by the present invention is that the existing direct-injection asphalt modifier is prepared by melt blending polymers such as SBS and additives, which may cause high-temperature processing loss and poor dispersibility of the modifier.

[0005] The present invention first prepares a microporous capsule shell by using a supercritical fluid pore-forming process for a polymer modifier, and then encapsulates a liquid modifier in the capsule by capillary action to prepare a solid-liquid integrated capsule asphalt modifier. The capsule asphalt modifier can quickly absorb asphalt into the pores in the asphalt due to its porous structure, and achieves uniform dispersion of the modifier phase during simple stirring.

[0006] A direct-cast capsule asphalt modifier comprises 10-50 parts by mass of a polymer capsule shell and 30-90 parts by mass of a liquid core agent; the liquid core agent is contained in the polymer capsule shell; the polymer capsule shell is porous, has a porosity greater than 90%, and a pore size of 0.05-500 μm.

[0007] The polymer capsule shell is prepared by using a supercritical fluid pore-making process.

[0008] The polymer capsule shell preparation process comprises the following steps:

[0009] S1. heating the polymer to a molten state;

[0010] S2. The porogen is heated and pressurized to a supercritical fluid state and then injected into the polymer melt in a certain mass ratio and stirred uniformly to obtain a molten blend;

[0011] S3. The molten blend is cooled to room temperature to obtain a polymer capsule shell.

[0012] The polymer includes one or any combination of two or more of polyethylene, polypropylene, oxidized polyethylene, oxidized polypropylene, SBS, SBR, EVA, POE, and polyolefin wax.

[0013] The porogen includes any one of carbon dioxide, nitrogen, ethanol and water.

[0014] The mass ratio of the porogen to the polymer melt is 0.003%-2%.

[0015] The capsule core agent includes any one of liquid asphalt, liquid epoxy resin, liquid acrylic resin, solvent oil, liquid antioxidant, coupling agent, and modifier dispersion.

[0016] The modifier dispersion includes any one of a carbon nanotube dispersion, a polyester fiber dispersion, and a calcium carbonate whisker dispersion.

[0017] A method for preparing a direct-cast capsule asphalt modifier comprises the following steps:

[0018] S1. The liquid core is added to the polymer capsule shell in a certain proportion to obtain a mixture;

[0019] S2. The mixture in step S1 was stirred at room temperature at a rate of 10-200 rpm for 10-200 min;

[0020] S3. After the stirring is completed, the finished product of the capsule asphalt modifier is obtained.

[0021] Beneficial Effects

[0022] 1. The capsule asphalt modifier uses microporous shell capsules to encapsulate the liquid modifier. The process is simple and does not require high-temperature processing, which avoids the loss of liquid modifiers during processing at high temperatures, thereby causing the formula ratio to fail. The solid-liquid integrated capsule asphalt modifier can be directly put into the asphalt tank or mixing plant. After simple stirring, the asphalt can be modified. No additional equipment is required, and it is easy to use.

[0023] 2. Capsule asphalt modifier has a developed void structure and ultra-high specific surface area. It can carry a certain amount of gas and be put into molten asphalt. The gas evaporates and foams the asphalt, reducing the viscosity of the asphalt, achieving a warm mix effect and reducing energy consumption.

[0024] 3. When the capsule asphalt modifier is put into the molten asphalt, the liquid modifier will quickly diffuse into the asphalt phase due to the concentration difference. At the same time, the liquid asphalt will be quickly adsorbed into the capsule shell. The asphalt and the modifier will be initially mixed. Then, the ultra-thin pore wall of the capsule will quickly melt in the hot asphalt. After simple stirring, it can be evenly dispersed in the asphalt phase, achieving the modification purpose and greatly improving the modification efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a physical photo of the capsule shell in Example 1;

[0026] Figure 2 Electron micrograph of capsule shell;

[0027] Figure 3 Preparation process of capsule asphalt modifier;

[0028] Figure 4 Capsule asphalt modifier photo;

[0029] Figure 5 Photo of the capsule asphalt modifier after being added to asphalt;

[0030] Figure 6 Morphological photos of the modifier prepared in Comparative Example 1;

[0031] Figure 7 Photo of the modifier added to asphalt in Comparative Example 1;

[0032] Figure 8 Photo of the modifier state in Comparative Example 2 DETAILED DESCRIPTION

[0033] The oxidized polyethylene used in the examples is NV-610P from Comino New Materials, the polypropylene is 1100N from PetroChina, the SBS is 1501 from Li Changrong, the SBR is QY52 from Qianyu, the EVA is 460 from DuPont, and the POE is 8003 from Dow Chemical.

[0034] The porogens used in the examples are nitrogen and carbon dioxide from Air Liquide.

[0035] The liquid core agent used in the examples is NPEL127 epoxy resin from Nanya Company, KN4006 oil from Xinjiang Karamay, carbon nanotube dispersion from Shenzhen Yite Technology Company, and KH-560 coupling agent from Hangzhou Jessica Chemical.

[0036] The 90# road petroleum asphalt used in the embodiment is Sinopec Donghai brand, and the 70# asphalt is Sichuan Hongyang.

[0037] Example 1

[0038] 2 kg SBS and 2 kg polypropylene were heated to 200 ° C, kept in a molten state and stirred evenly. At the same time, 5 g carbon dioxide was heated to 60 ° C, pressurized to 9 MPa to form a supercritical fluid, injected into the polypropylene melt, stirred evenly, and then cooled to obtain a microporous capsule shell. Its SEM photo is shown as follows: Figure 1 As shown;

[0039] 1 kg of microporous capsule shell and 1 kg of epoxy resin were mixed evenly to obtain a granular capsule asphalt modifier;

[0040] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 70# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0041] The specific performance tests are shown below.

[0042]

[0043] Example 2

[0044] 2kg SBR and 2kg oxidized polypropylene were heated to 180°C, kept in a molten state and stirred evenly, and at the same time, 10g nitrogen was heated to 60°C, pressurized to 7MPa to form a supercritical fluid, injected into the polymer melt, stirred evenly, and then cooled to obtain a microporous capsule shell;

[0045] 1 kg of microporous capsule shell and 6 kg of KN4006 oil were mixed evenly to obtain a granular capsule asphalt modifier;

[0046] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 70# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0047] The specific performance tests are shown below.

[0048]

[0049] Example 3

[0050] 3kg EVA was heated to 200°C and stirred evenly while being kept in a molten state. Meanwhile, 50g carbon dioxide was heated to 60°C and pressurized to 9MPa to form a supercritical fluid, which was injected into the polymer melt, stirred evenly, and then cooled to obtain a microporous capsule shell.

[0051] 1 kg of microporous capsule shell and 0.6 kg of carbon nanotube dispersion were mixed evenly to obtain a granular capsule asphalt modifier;

[0052] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 70# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0053] The specific performance tests are shown below.

[0054]

[0055]

[0056] Example 4

[0057] 2kg POE and 0.5kg polypropylene were heated to 200°C, kept in a molten state and stirred evenly, and 20g carbon dioxide was heated to 60°C, pressurized to 9MPa to form a supercritical fluid, injected into the polymer melt, stirred evenly, and then cooled to obtain a microporous capsule shell;

[0058] 1 kg of microporous capsule shell and 0.8 kg of KH560 coupling agent fat were mixed evenly to obtain a granular capsule asphalt modifier;

[0059] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 90# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0060] The specific performance tests are shown below.

[0061]

[0062] Example 5

[0063] 1kg SBS, 0.5kg polypropylene and 0.5kg EVA were heated to 200°C, kept in a molten state and stirred evenly, and 35g carbon dioxide was heated to 60°C, pressurized to 9MPa to form a supercritical fluid, injected into the polypropylene melt, stirred evenly, and then cooled to obtain a microporous capsule shell;

[0064] 1 kg of microporous capsule shell and 1.5 kg of KN4006 oil were mixed evenly to obtain a granular capsule asphalt modifier;

[0065] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 90# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0066] The specific performance tests are shown below.

[0067]

[0068] Comparative Example 1

[0069] The scheme using direct melt mixing is as follows:

[0070] 2 kg of SBS and 2 kg of polypropylene were heated to 200°C, stirred evenly while maintaining the molten state, and then cooled to obtain blended polymer particles;

[0071] 1 kg of polymer particles and 1 kg of epoxy resin were mixed evenly to obtain an asphalt modifier;

[0072] Add 140g of the above modifier into 860g of 70# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0073] The overall morphology of the obtained modifier is a two-phase mixture of plastic particles and liquid additives, such as Figure 6 Shown

[0074] The modifier prepared in Comparative Example 1 was added to asphalt. The modifier was difficult to melt and floated on the surface of the asphalt in the form of particles. The photo of the modified asphalt obtained is shown in Figure 7. It can be seen that the modifier is poorly soluble in asphalt and has poor dispersibility. Figure 5 There are significant differences.

[0075] The specific test comparison performance is as follows

[0076]

[0077] The polymer melt has not been pore-formed by supercritical fluid, and there is no pore structure in its particles, so it cannot absorb liquid additives. In addition, when the non-porous polymer particles are added to asphalt, it is difficult to melt quickly and form a homogeneous phase with the asphalt. The porous structure of the capsule carrier in the present invention increases the contact surface between the asphalt and the polymer, and the asphalt can quickly enter the capsule and then melt into a homogeneous phase.

[0078] Comparative Example 2

[0079] The traditional method of preparing the modifier by blending and granulation is as follows:

[0080] 2kg of SBR, 2kg of oxidized polypropylene and 24kg of KN4006 oil were uniformly mixed, and then extruded and granulated through a screw extruder to obtain a modifier.

[0081] Add 140g of the above-mentioned capsule asphalt modifier into 860g of 70# asphalt at a temperature of 170°C, and then stir at a speed of 100rpm for 30min to obtain modified asphalt.

[0082] The specific test comparison performance is as follows

[0083]

[0084] It is difficult to prepare a modifier formula with a high content of liquid additives using the traditional blending and granulation process. The prepared high liquid content formula modifier cannot be formed. Although it can be quickly melted when added to asphalt, the performance of the modified asphalt is still slightly poor. This is mainly because the dispersion uniformity of this amorphous colloidal modifier is still worse than that of the capsule modifier.

Claims

1. An application of a direct-cast capsule asphalt modifier in the preparation of modified asphalt that can quickly enter the capsule and then melt into a homogeneous phase, characterized in that: The direct-cast capsule asphalt modifier comprises 10-50 parts by mass of a polymer capsule shell and 30-90 parts by mass of a liquid core agent; the liquid core agent is contained in the polymer capsule shell; the polymer capsule shell is porous, and the porosity is greater than 90%, and the pore size is 0.05-500 μm; The polymer capsule shell is prepared by a supercritical fluid pore-making process; The polymer capsule shell preparation process comprises the following steps: S1. heating the polymer to a molten state; S2. The porogen is heated and pressurized to a supercritical fluid state and then injected into the polymer melt in a certain mass ratio and stirred uniformly to obtain a molten blend; S3. The molten blend is cooled to room temperature to obtain a polymer capsule shell; The polymer includes one or any combination of two or more of oxidized polyethylene, polypropylene, SBS, SBR, EVA, and POE; The porogen includes any one of carbon dioxide, nitrogen, ethanol and water; The mass ratio of the porogen to the polymer melt is 0.003-2%; The capsule core agent includes liquid epoxy resin; The preparation method of the direct-cast capsule asphalt modifier comprises the following steps: S1. Add the liquid core agent into the polymer capsule shell in a certain proportion to obtain a mixture; S2. Stir the mixture in step S1 at room temperature at a rate of 10-200 rpm for 10-200 min; S3. After the stirring is completed, the finished capsule asphalt modifier is obtained.