A method for preparing low-oxygen rare earth alloy cored wire blank
Preparing low-oxygen rare earth alloy cored wire blanks through molten salt electrolysis and negative pressure transfer methods solves the problem of high oxygen content in rare earth steel and realizes low-oxygen content rare earth alloy cored wire blanks, simplifying the preparation process and reducing costs. cost, and has the prospect of large-scale industrial production.
Patent Information
- Application Number
- CN202310086779.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-17
AI Technical Summary
The high oxygen content in existing rare earth steel results in serious burning loss of rare earth elements and low yield. The preparation process of low-oxygen rare earth additives is cumbersome, making it difficult to achieve large-scale industrial production.
Molten salt electrolysis and negative pressure transfer methods are used to prepare low-oxygen rare earth alloy cored wire blanks. Molten salt electrolysis is performed through rare earth oxides and rare earth fluorides, and the alloy liquid is cooled and formed using a negative pressure transfer device to control the oxygen content below 0.008wt. .%.
The low oxygen content of the rare earth alloy cored wire blank is achieved, the preparation process is simplified, the cost is reduced, it has continuous production capability, the product composition is uniform, and the oxidation resistance is enhanced.
Smart Images

Figure CN116083684B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth alloys, and in particular to a method for preparing a low-oxygen rare earth alloy cored wire blank. Background Art
[0002] As we all know, adding rare earth to steel can deeply remove oxygen and sulfur, micro-alloy and refine grains, and improve mechanical properties and corrosion resistance. However, due to the strong activity of rare earth, which is second only to alkali metals and alkaline earth metals, and has a lower specific gravity than steel, adding rare earth to molten steel above 1500℃ will cause serious burnout of rare earth and very low yield. In addition, the occurrence state of rare earth elements in steel is unstable, resulting in unstable performance of rare earth steel. It even reacts with the continuous casting nozzle to cause nodules, which brings negative effects.
[0003] The effect of rare earth addition is closely related to the cleanliness of molten steel, the method of rare earth addition, and the stability of the application environment (refractory materials, metallurgical slag). For a long time in the past, the research focus of rare earth steel was mainly on reducing the oxygen content of molten steel. As the purity of molten steel has become higher and higher, in recent years, people have begun to pay attention to the oxygen content in rare earths. The oxygen content in rare earths also has a great influence on the size and shape of rare earth inclusions, which in turn affects the effect of rare earth addition. Chinese patent CN106756446A proposes a method for preparing a rare earth iron intermediate alloy for low-oxygen rare earth steel, and Chinese patent CN113134596A proposes a method for preparing low-oxygen rare earth wire, but the oxygen content is greater than 0.04%. In general, the preparation method of low-oxygen rare earth additives reported has a long process and cumbersome steps, which is difficult to large-scale industrial production.
[0004] At present, rare earth steel additives include single rare earth metals and mixed rare earth metals, and their shapes include blocks, ingots, wires, powders, rods, or cored wires filled with rare earth powder. However, a mature method of rare earth addition that can be commercialized on a large scale has not yet been explored. The rare earth cored wire is fed into the molten steel through a wire feeder. The outer metal shell of the rare earth wire can play a role similar to a "capsule", feeding the rare earth wire into the specified position in the molten steel, effectively avoiding the reaction with air and slag, reducing the burning of active alloy elements, and having a higher rare earth absorption rate and a more stable addition effect. However, the current difficulty in preparing low-oxygen rare earth wires or cored wires is much greater than that of rare earth blocks or rare earth rods. Summary of the invention
[0005] The purpose of the embodiment of the present invention is to provide a method for preparing a low-oxygen rare earth alloy cored wire blank, in which a rare earth alloy solution with a low oxygen content is obtained by molten salt electrolysis and negative pressure transfer, and the solution is placed in an inert gas for natural cooling, thereby achieving a low oxygen content in the cored wire blank, and having the advantages of short preparation process, low cost, and strong continuous production capacity.
[0006] In order to solve the above technical problems, an embodiment of the present invention provides a method for preparing a low-oxygen rare earth alloy cored wire blank, comprising the following steps:
[0007] Molten salt electrolysis is carried out using rare earth oxides as raw materials, rare earth fluorides as electrolytes, and alkali metal and alkaline earth metal fluorides as additives to the electrolyte to obtain a rare earth alloy liquid, wherein the operating temperature of the electrolytic cell is a first preset temperature, the operating time of the electrolytic cell is a first preset time, the average current intensity is a first preset current value, the rare earth oxides include: at least one of cerium oxide, neodymium oxide, lanthanum oxide, praseodymium oxide, and yttrium oxide, the rare earth fluorides are fluorides of the same rare earth element, the alkali metal and alkaline earth metal fluorides are lithium fluoride and barium fluoride, and the sum of the oxygen contents in the materials of the cathode and crucible of the electrolytic equipment is less than or equal to the first preset ratio value.
[0008] The rare earth alloy liquid is transferred from the electrolysis device to the cored wire blank mold based on a negative pressure transfer device, wherein the internal vacuum degree of the negative pressure transfer device is less than a first preset pressure value;
[0009] The rare earth alloy liquid in the cored wire blank mold is placed in an inert gas environment and cooled naturally to obtain a low-oxygen rare earth alloy cored wire blank.
[0010] Furthermore, before preparing the rare earth oxides and rare earth fluorides by molten salt electrolysis, the method further comprises:
[0011] Removing free water and crystal water from the rare earth oxide raw material and the rare earth fluoride, alkali metal and alkaline earth metal fluoride;
[0012] The cathode, crucible, straw, guide tube, buffer tank and cored wire blank mold in the electrolysis equipment are baked at a second preset temperature and for a second preset duration.
[0013] Further, the numerical range of the second preset temperature is 200°C-500°C;
[0014] The numerical range of the second preset time length is 8h-12h.
[0015] Further, the numerical range of the first preset temperature is 950°C-1100°C;
[0016] The numerical range of the first preset duration is 200min-350min;
[0017] The numerical range of the first preset current value is 3000A-4000A;
[0018] The first preset ratio value is 0.10wt%;
[0019] The first preset pressure value is 0.1 kPa.
[0020] Furthermore, the negative pressure transfer device comprises: a suction pipe, a negative pressure cavity, a guide tube, a heating jacket, a vacuum pump, and a buffer tank;
[0021] One end of the straw is connected to the rare earth alloy liquid pool in the electrolysis equipment, and the other end is connected to the negative pressure cavity and one end of the guide tube respectively;
[0022] The other end of the guide tube is connected to a plurality of cored wire blank molds through the buffer tank;
[0023] The air inlet of the negative pressure cavity is connected to the air source, and the air outlet is connected to the vacuum pump;
[0024] Wherein, the gas source is an inert gas, and its oxygen content is less than ≤10ppm.
[0025] The heating jacket is used to heat the straw and the guide tube, and the heating temperature is 900-1100°C.
[0026] Furthermore, the connection end of the straw with the rare earth alloy liquid pool is lower than the connection end with the negative pressure cavity;
[0027] The inclination angle of the straw is greater than or equal to a first preset angle value;
[0028] The numerical range of the first preset angle value is 15°-25°.
[0029] Furthermore, the sum of the volumes of the buffer tank and the plurality of cored wire blank molds is greater than the sum of the volumes of the negative pressure cavity, the suction tube, and the guide tube.
[0030] Further, the material of the cored wire blank mold is one of pure iron, low carbon steel, stainless steel tube, titanium alloy tube, and nickel alloy tube, and its oxygen content is ≤0.01wt.%;
[0031] The outer diameter of the cored wire blank mold has a numerical range of 20 mm to 50 mm, the wall thickness has a numerical range of 3 mm to 6 mm, and the length has a numerical range of 0.4 m to 1.2 m;
[0032] Preferably, the outer diameter of the cored wire blank has a numerical range of 25 mm to 30 mm, and the length of the cored wire blank has a numerical range of 0.5 m to 1 m.
[0033] Furthermore, the rare earth in the rare earth alloy liquid accounts for 60wt.%-98wt.%, and the rare earth includes one or more of lanthanum, cerium, praseodymium, neodymium, and yttrium;
[0034] The balance of the rare earth alloy liquid includes one or more of iron, titanium, and cobalt, or the balance of the rare earth alloy includes one or more of aluminum and magnesium.
[0035] Furthermore, the relationship coefficient k between the mass of rare earth oxides and rare earth fluorides input in the molten salt electrolysis preparation process and the mass of the output rare earth products is:
[0036] k=1.02~1.05,
[0037] in, m1 is the mass of rare earth elements in the rare earth oxide, m2 is the mass of rare earth elements in the rare earth fluoride, and m3 is the mass of rare earth elements in the rare earth product.
[0038] The above technical solution of the embodiment of the present invention has the following beneficial technical effects:
[0039] First, the preparation process of rare earth alloy cored wire blank is short, the cost is low, and continuous production is possible; second, the low oxygen content of rare earth cored wire blank is easy to control, so that the oxygen content of the final cored wire product is low, and the effect of adding it to steel is significant; third, the composition of the rare earth alloy cored wire blank is uniform and there is no segregation; fourth, the presence of iron, aluminum, magnesium, titanium, and cobalt elements in the rare earth alloy cored wire increases its oxidation resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is a flow chart of a method for preparing a low-oxygen rare earth alloy cored wire blank provided by an embodiment of the present invention;
[0041] Figure 2 It is a schematic diagram of the principle of the negative pressure transfer device provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0043] Please refer to Figure 1 The embodiment of the present invention provides a method for preparing a low-oxygen rare earth alloy cored wire blank, comprising the following steps:
[0044] Step S300, using rare earth oxide as raw material, rare earth fluoride as electrolyte, alkali metal and alkaline earth metal fluoride as additives of the electrolyte, to carry out molten salt electrolysis to obtain rare earth alloy liquid, wherein the working temperature of the electrolytic cell is a first preset temperature, the working time of the electrolytic cell is a first preset time, the average current intensity is a first preset current value, the rare earth oxide includes: at least one of cerium oxide, neodymium oxide, lanthanum oxide, praseodymium oxide, and yttrium oxide, the rare earth fluoride is a fluoride of the same rare earth element, the alkali metal and alkaline earth metal fluoride are lithium fluoride, barium fluoride, and the sum of the oxygen contents in the cathode and crucible of the electrolysis equipment is less than or equal to the first preset ratio value.
[0045] Specifically, the first preset ratio value is 0.10wt%;
[0046] Furthermore, the relationship coefficient k between the quality of rare earth oxides and rare earth fluorides input in the molten salt electrolysis preparation process and the quality of the output rare earth products is:
[0047] k=1.02~1.05,
[0048] in, m1 is the mass of rare earth elements in rare earth oxides, m2 is the mass of rare earth elements in rare earth fluorides, and m3 is the mass of rare earth elements in rare earth products.
[0049] Step S400, transferring the rare earth alloy liquid from the electrolysis equipment to the cored wire blank mold based on a negative pressure transfer device, wherein the internal vacuum degree of the negative pressure transfer device is less than a first preset pressure value.
[0050] Specifically, the numerical range of the first preset temperature is 950°C-1100°C; the numerical range of the first preset time is 200min-350min; the numerical range of the first preset current value is 3000A-4000A; and the first preset pressure value is 0.1kPa.
[0051] Step S500, placing the rare earth alloy liquid in the cored wire blank mold in an inert gas environment for natural cooling to obtain a low-oxygen rare earth alloy cored wire blank.
[0052] The cored wire blank mold filled with rare earth alloy liquid is removed, and replaced with an empty cored wire blank mold to continue suction and continuous production. The removed cored wire blank mold is naturally cooled in an inert protective atmosphere.
[0053] In addition, in order to further reduce the oxygen content, the following measures can be taken: reduce the amount of rare earth oxide added by 20% to 50% in the time interval of 30 to 50 minutes before the transfer of the rare earth alloy liquid, increase the distance between the cathode and the anode by 3 to 8 cm, increase the temperature of the electrolytic cell by 30 to 70°C, and double the amount of lithium fluoride additive. In the specific preparation process, one or more of the above measures can be selected.
[0054] The traditional method of preparing rare earth iron alloys by doping requires obtaining a single pure rare earth metal, and the metal thermal reduction method requires a reducing agent, which is costly, and it is also necessary to make metal rods first, draw them into wires, and then coat them with metal layers to make cored wires. The process is cumbersome and the preparation cycle is long. In the present invention, the molten rare earth alloy obtained by molten salt electrolysis is directly pumped into a specific cored wire blank mold, and the cored wire blank obtained after cooling can be directly supplied to downstream cored wire companies for use, which saves a lot of processes, effectively avoids secondary pollution, has a simple process, can be produced continuously, has low cost, and has the prospect of large-scale industrial production.
[0055] The oxygen content of the rare earth alloy prepared by molten salt electrolysis can be controlled within 0.008wt.%. The low-oxygen raw materials ensure that the oxygen content of the final rare earth alloy cored wire product is low (≤0.03wt.%), reducing the formation of high-melting-point inclusions in molten steel, thereby meeting the rare earth addition requirements.
[0056] Rare earth alloys prepared by doping and metal thermal reduction methods have serious segregation problems. A major advantage of rare earth alloys prepared by molten salt electrolysis is that the composition and structure are very uniform and there is no segregation. The rare earth alloy cored wire blank can be better drawn into wire without breaking.
[0057] Furthermore, before preparing the rare earth oxides and rare earth fluorides by molten salt electrolysis in step S300, the process further includes:
[0058] Step S100, removing free water and crystal water from rare earth oxide raw materials, rare earth fluorides, and alkali metals and alkaline earth metal fluorides.
[0059] Step S200, baking the cathode, crucible, straw, guide tube, buffer tank and cored wire blank mold in the electrolysis equipment, the baking temperature is a second preset temperature, and the baking time is a second preset duration.
[0060] Specifically, the numerical range of the second preset temperature is 200° C.-500° C.; the numerical range of the second preset time is 8h-12h.
[0061] For details, please refer to Figure 2The negative pressure transfer device used in step S400 includes: a straw, a negative pressure cavity, a guide tube, a heating sleeve, a vacuum pump, and a buffer tank; one end of the straw is connected to the rare earth alloy liquid pool in the electrolysis equipment, and the other end is respectively connected to the negative pressure cavity and one end of the guide tube; the other end of the guide tube is respectively connected to a plurality of cored wire blank molds through the buffer tank; the air inlet of the negative pressure cavity is connected to the air source, and the air outlet thereof is connected to the vacuum pump; the heating sleeve is used to heat the straw and the guide tube, and the heating temperature is 900-1100°C; wherein the gas source is an inert gas, and its oxygen content is less than ≤10ppm.
[0062] Furthermore, the materials of the straw, negative pressure chamber and guide tube should be high temperature resistant and non-polluting materials. The straw and guide tube preferably have a circular cross-section and a smooth inner wall; the inner diameter of the straw d1 = 15 ~ 30mm, and the inner diameter of the guide tube d2 = (1.3 ~ 1.5) d1; when transferring liquid, the vacuum degree p in the negative pressure chamber is ≤ 0.1kPa.
[0063] Furthermore, the connection end of the straw with the rare earth alloy liquid pool is lower than the connection end with the negative pressure cavity; the inclination angle of the straw is greater than or equal to a first preset angle value. Specifically, the numerical range of the first preset angle value is 15°-25°.
[0064] Furthermore, the sum of the volumes of the buffer tank and several cored wire blank molds is greater than the sum of the volumes of the negative pressure cavity, the suction pipe and the guide tube. That is, in the solidification molding process, the mold should be made of a material that is resistant to high temperatures and does not pollute the product, preferably the metal layer material of claim 1; the relationship between the volume V1 of the (buffer tank + cored wire blank cavity), the volume V2 of the negative pressure cavity, the volume V3 of the suction pipe, and the volume V4 of the guide tube satisfies: V1≥1.2(V2+V3+V4).
[0065] Furthermore, the cored wire blank mold is made of one of pure iron, low carbon steel, stainless steel tube, titanium alloy tube, and nickel alloy tube, and its oxygen content is ≤0.01wt.%. The outer diameter of the cored wire blank mold ranges from 20mm to 50mm, the wall thickness ranges from 3mm to 6mm, and the length ranges from 0.4m to 1.2m.
[0066] Preferably, the outer diameter of the cored wire blank has a numerical range of 25 mm to 30 mm, and the length of the cored wire blank has a numerical range of 0.5 m to 1 m.
[0067] Furthermore, the rare earth content in the rare earth alloy liquid is 60wt.%-98wt.%, and the rare earth includes one or more of lanthanum, cerium, praseodymium, neodymium, and yttrium; the balance of the rare earth alloy liquid includes one or more of iron, titanium, and cobalt, or the balance of the rare earth alloy includes one or more of aluminum and magnesium.
[0068] Specifically, in the rare earth alloy, the rare earth accounts for 60-98wt.%, selected from one or more of lanthanum, cerium, praseodymium, neodymium, and yttrium, and the proportion is arbitrary, preferably one or more of lanthanum, cerium, and yttrium, and the remainder is one or more of iron, titanium, and cobalt, and the proportion is arbitrary, or one or more of aluminum and magnesium, and the proportion is arbitrary.
[0069] Specifically, the selection of rare earth elements includes: lanthanum, cerium, praseodymium, neodymium, and yttrium, all of which are rare earth elements that can be easily achieved by molten salt electrolysis, and the process is relatively mature. One or more of lanthanum, cerium, and yttrium are preferred, mainly considering that these three elements are commonly added elements to rare earth steel, and are relatively cheap and highly abundant.
[0070] Specifically, the selection of other metal elements includes: introducing one or more of iron, aluminum, magnesium, titanium, and cobalt into rare earth alloys. First, the alloys composed of these elements and rare earths are easily obtained by molten salt electrolysis; second, the introduction of aluminum, magnesium, titanium, and cobalt into rare earth alloys can make the final product - rare earth cored wire added to steel, play a role in microalloying, among which aluminum and magnesium are strong deoxidizers, which can further purify the molten steel. Third, the introduction of iron, aluminum, magnesium, titanium, and cobalt into rare earth alloys can enhance the corrosion and oxidation resistance of rare earth cored wire blanks. The activity of rare earth elements is second only to alkali metals and is equivalent to that of alkaline earth metals. The introduction of iron, aluminum, magnesium, titanium, and cobalt elements can enhance the antioxidant properties of rare earth elements and facilitate storage and transportation.
[0071] In the low-oxygen rare earth alloy cored wire blank obtained by the above preparation method, the oxygen content of the core of the cored wire blank is ≤0.008wt.%, preferably ≤0.005wt.%, carbon content ≤0.05wt.%, phosphorus content ≤0.01wt.%, and sulfur content ≤0.005wt.%.
[0072] Low-oxygen rare earth alloy cored wire blanks are the key to ensuring low oxygen in the final cored wire product. Low oxygen in rare earth additives is also a key indicator that affects the smooth casting process of rare earth steel and the properties of rare earth steel. Compared with block and rod-shaped rare earth additives, it is very difficult to achieve low oxygen in rare earth wires or cored wires. The oxygen content in rare earth cored wires on the market is generally above 500ppm, and there is a huge gap in the market demand for low-oxygen rare earth cored wires. The technical solution of the present invention starts from strictly controlling the oxygen content in the rare earth alloy cored wire blank, and proposes a method for preparing a low-oxygen (≤0.008wt.%) rare earth cored wire blank. Based on the low-oxygen cored wire blank, the prepared rare earth cored wire can achieve an oxygen content of ≤0.03wt.%, with excellent performance and meeting market demand.
[0073] The above preparation method is described in detail with several embodiments below:
[0074] Example 1
[0075] A pure iron rod is used as a consumable cathode, graphite is used as an anode, and the purity of cerium oxide after removing free water and crystal water is 99.99%. The raw material is cerium fluoride and lithium fluoride. The working temperature of the electrolytic cell is controlled at about 980°C, and the average current intensity is 4000A. After 200 minutes of electrolysis, the ferrocerium alloy liquid is pumped into a cored wire blank mold with an outer diameter of 20mm and a wall thickness of 3mm by means of a negative pressure suction device. The mold material is pure iron, wherein the inner diameter of the suction pipe of the suction device is d1=15mm, and the inner diameter of the guide pipe is d2=19.5mm; when transferring the liquid, the vacuum degree in the negative pressure cavity is 0.1kPa, the inclination angle β of the suction pipe is 15°, and the heating temperature of the heating sleeve is 980°C. After thorough cooling, the element content in the cored wire blank is tested as shown in the following table:
[0076] Table 1 Example 1 Core wire blank composition (wt.%)
[0077] What Fe O C P S And min 60.00 39.86 0.0050 0.01 <0.001 <0.001 <0.01 <0.005
[0078] Comparative Example 1
[0079] Ferrocerium metal of the same mass ratio as in Example 1 was weighed, melted and mixed in a vacuum induction furnace by a counter-blending method, and cast into a rod with an outer diameter of 17 mm. After solidification and cooling, a pure iron shell with an outer diameter of 20 mm and a wall thickness of 3 mm was put on to make a cored wire blank. After testing, it was found that the oxygen content in the core was 0.024wt.%, which was significantly higher than that in Example 1.
[0080] Example 2
[0081] The iron rod is used as the consumable cathode, graphite is used as the anode, the purity of neodymium oxide and lanthanum oxide mixture after removing free water and crystal water is 99.99% as the raw material, the electrolyte is neodymium fluoride, lanthanum fluoride, lithium fluoride, the average current intensity is 3000A, the working temperature of the electrolytic cell is controlled at about 1100℃, and after 350min of electrolysis, the alloy liquid is pumped into the cored wire blank mold with an outer diameter of 30mm and a wall thickness of 4mm by means of a negative pressure suction device. The mold material is stainless steel, where the inner diameter of the suction pipe of the suction device is d1=20mm, and the inner diameter of the guide pipe is d2=30mm; when transferring the liquid, the vacuum degree in the negative pressure cavity is 80Pa, the inclination angle β of the suction pipe is 18°, and the heating temperature of the heating sleeve is 1100℃. After thorough cooling, the element content in the cored wire blank is tested as shown in the following table:
[0082] Table 2 Example 2 Core wire blank composition (wt.%)
[0083]
[0084]
[0085] Example 3
[0086] Pure cobalt rods were used as consumable cathodes, graphite was used as anodes, the purity of free water and crystal water was 99.99%, praseodymium oxide was used as raw material, praseodymium fluoride and lithium fluoride were used as electrolytes, the working temperature of the electrolytic cell was controlled at about 1000°C, the average current intensity was 3800A, and after 300 minutes of electrolysis, the alloy liquid was pumped into a cored wire blank mold with an outer diameter of 40mm and a wall thickness of 4mm by means of a negative pressure suction device. The mold material was nickel alloy, wherein the inner diameter of the suction pipe of the suction device was d1 = 25mm, and the inner diameter of the guide pipe was d2 = 35mm; when transferring the liquid, the vacuum degree in the negative pressure cavity was 60Pa, the inclination angle β of the suction pipe was 20°, and the heating temperature of the heating sleeve was 1000°C. After thorough cooling, the element content in the cored wire blank was tested as shown in the following table:
[0087] Table 3 Example 3 Core wire blank composition (wt.%)
[0088] Pr Co. O C P S And min 98.0 1.85 0.0044 0.009 <0.001 <0.001 <0.01 <0.005
[0089] Example 4
[0090] Titanium-iron alloy rods are used as consumable cathodes, graphite is used as anodes, and the purity of cerium oxide after removing free water and crystal water is 99.99%. The electrolyte is cerium fluoride and lithium fluoride. The working temperature of the electrolytic cell is controlled at about 1100°C, and the average current intensity is 3900A. After 350 minutes of electrolysis, the alloy liquid is pumped into the cored wire blank mold with an outer diameter of 33mm and a wall thickness of 4mm by means of a negative pressure suction device. The mold material is titanium alloy, where the inner diameter of the suction pipe of the suction device is d1=30mm, and the inner diameter of the guide pipe is d2=45mm; when transferring the liquid, the vacuum degree in the negative pressure cavity is 30Pa, the inclination angle β of the suction pipe is 22°, and the heating temperature of the heating sleeve is 1050°C. After thorough cooling, the element content in the cored wire blank is tested as shown in the following table:
[0091] Table 4 Example 4 Core wire blank composition (wt.%)
[0092] What Fe IT O C P S And min 65.13 20.36 14.39 0.0038 0.017 <0.001 <0.001 <0.01 <0.005
[0093] Example 5
[0094] With tungsten rod as cathode and graphite as anode, the purity of yttrium oxide and magnesium oxide after removing free water and crystal water is 99.99% as raw materials, the electrolyte is yttrium fluoride and lithium fluoride, the average current intensity is 3300A, the working temperature of the electrolytic cell is controlled at about 1080℃, and after 250min of electrolysis, the magnesium-yttrium alloy liquid is pumped into the cored wire blank mold with an outer diameter of 25mm and a wall thickness of 3.5mm by means of a negative pressure suction device. The mold material is low carbon steel, where the inner diameter of the suction pipe of the suction device is d1=20mm, and the inner diameter of the guide pipe is d2=30mm; when transferring the liquid, the vacuum degree in the negative pressure cavity is 80Pa, the inclination angle β of the suction pipe is 18°, and the heating temperature of the heating sleeve is 1080℃. After thorough cooling, the element content in the cored wire blank was tested as shown in the following table:
[0095] Table 5 Example 5 Core wire blank composition (wt.%)
[0096] Y Mg O C P S And min 87.03 12.83 0.0045 0.015 <0.001 <0.001 <0.01 <0.005
[0097] Example 6
[0098] With tungsten rod as cathode and graphite as anode, the purity of lanthanum oxide, cerium oxide, neodymium oxide and praseodymium oxide after removing free water and crystal water is 99.99%. The electrolyte is cryolite and alumina. The average current intensity is 4000A. The working temperature of the electrolytic cell is controlled at about 950℃. After 350min of electrolysis, the alloy liquid is pumped into the cored wire blank mold with an outer diameter of 25mm and a wall thickness of 3.5mm by means of a negative pressure suction device. The mold material is low carbon steel, where the inner diameter of the suction pipe of the suction device is d1 = 20mm, and the inner diameter of the guide pipe is d2 = 30mm; when transferring the liquid, the vacuum degree in the negative pressure cavity is 20Pa, the inclination angle β of the suction pipe is 25°, and the heating temperature of the heating sleeve is 900℃. After thorough cooling, the element content in the cored wire blank is tested as shown in the following table:
[0099] Table 6 Example 6 Core wire blank composition (wt.%)
[0100] to What Pr when Al O C P S And min 33.23 18.31 5.45 10.74 32.15 0.0029 0.02 <0.001 <0.001 <0.01 <0.005
[0101] Example 7
[0102] The ferrocerium alloy cored wire blank obtained in Example 1 was drawn into a cored wire with a diameter of 5 mm, and the oxygen in the core was tested to be 0.027 wt.%. It was added to the molten steel from the tundish through the wire feeder, and it was found that the addition process did not soften and could penetrate into the molten steel. The final yield of rare earth cerium in the steel was 58%, and the mechanical properties and corrosion resistance of the steel were significantly improved. Moreover, the nozzle nodule phenomenon was not obvious after continuous casting for 500 minutes, and the process was smooth.
[0103] Comparative Example 2
[0104] The ferrocerium alloy cored wire blank obtained in Comparative Example 1 was drawn into a cored wire with a diameter of 5 mm, and the oxygen in the core was tested to be 0.06 wt.%. The ferrocerium alloy cored wire was added to the molten steel from the tundish through the wire feeder, and the yield of rare earth cerium in the steel was 48%. After continuous casting for 260 minutes, the nozzle was severely lumped and the pouring was stopped.
[0105] Example 8
[0106] The lanthanum-neodymium-iron alloy cored wire blank obtained in Example 2 was drawn into a cored wire with a diameter of 8 mm, and the oxygen in the core was tested to be 0.025 wt.%. It was added to the molten steel from the tundish through the wire feeder, and it was found that the addition process did not soften and could penetrate into the molten steel. Finally, the yield of rare earth cerium in the steel was 65%, and the mechanical properties and corrosion resistance of the steel were significantly improved. The nozzle nodule phenomenon was not obvious after continuous casting for 600 minutes, and the process was smooth.
[0107] The embodiment of the present invention is intended to protect a method for preparing a low-oxygen rare earth alloy cored wire blank, comprising the following steps: using rare earth oxide as a raw material, using rare earth fluoride as an electrolyte, and using alkali metal and alkaline earth metal fluoride as additives of the electrolyte to perform molten salt electrolysis to obtain a rare earth alloy liquid, wherein the working temperature of the electrolytic cell is a first preset temperature, the working time of the electrolytic cell is a first preset time, the average current intensity is a first preset current value, and the rare earth oxide is at least one of cerium oxide, neodymium oxide, lanthanum oxide, praseodymium oxide, and yttrium oxide. , the rare earth fluoride is the fluoride of the same rare earth element, the alkali metal and alkaline earth metal fluoride is lithium fluoride and barium fluoride, the sum of the oxygen content in the material of the cathode and crucible of the electrolysis equipment is less than or equal to the first preset ratio value; the rare earth alloy liquid is transferred from the electrolysis equipment to the cored wire blank mold based on the negative pressure transfer device, wherein the internal vacuum degree of the negative pressure transfer device is less than the first preset pressure value; the rare earth alloy liquid in the cored wire blank mold is placed in an inert gas environment and cooled naturally to obtain a low-oxygen rare earth alloy cored wire blank. The above technical solution has the following effects:
[0108] First, the preparation process of the rare earth alloy cored wire blank is short, the cost is low, and continuous production is possible; second, the low oxygen content of the rare earth cored wire blank of the present invention is easy to control, so that the oxygen content of the final cored wire product is low, and the effect of adding it to steel is significant; third, the composition of the obtained rare earth alloy cored wire blank is uniform and non-segregated; fourth, the presence of iron, aluminum, magnesium, titanium, and cobalt elements in the rare earth alloy cored wire increases oxidation resistance.
[0109] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A method for preparing a low-oxygen rare earth alloy cored wire blank, characterized in that: The steps include: Using rare earth oxide as a raw material, using rare earth fluoride as an electrolyte, using alkali metal fluoride and alkaline earth metal fluoride as additives to the electrolyte, molten salt electrolysis is performed to obtain a rare earth alloy liquid, wherein the working temperature of the electrolytic cell is a first preset temperature, the working time of the electrolytic cell is a first preset time, the average current intensity is a first preset current value, the rare earth oxide is at least one of cerium oxide, neodymium oxide, lanthanum oxide, praseodymium oxide, and yttrium oxide, the rare earth fluoride is a fluoride of the same rare earth element, the alkali metal fluoride and alkaline earth metal fluoride are lithium fluoride and barium fluoride, and the sum of the oxygen content in the material of the cathode and crucible of the electrolytic equipment is less than or equal to the first preset ratio value; The rare earth alloy liquid is transferred from the electrolysis device to the cored wire blank mold based on a negative pressure transfer device, wherein the internal vacuum degree of the negative pressure transfer device is less than a first preset pressure value; Placing the rare earth alloy liquid in the cored wire blank mold in an inert gas environment and cooling it naturally to obtain a low-oxygen rare earth alloy cored wire blank; The negative pressure transfer device comprises: a suction pipe, a negative pressure cavity, a flow guide pipe, a heating jacket, a vacuum pump, and a buffer tank; One end of the straw is connected to the rare earth alloy liquid pool in the electrolysis equipment, and the other end is connected to the negative pressure cavity and one end of the guide tube respectively; The other end of the guide tube is connected to a plurality of cored wire blank molds through the buffer tank; The air inlet of the negative pressure cavity is connected to the air source, and the air outlet is connected to the vacuum pump; The heating jacket is used to heat the straw and the guide tube; The connection end of the straw with the rare earth alloy liquid pool is lower than the connection end with the negative pressure cavity; The inclination angle of the straw is greater than or equal to a first preset angle value; The numerical range of the first preset angle value is 15°-25°; The numerical range of the first preset temperature is 950°C-1100°C; The numerical range of the first preset duration is 200min-350min; The numerical range of the first preset current value is 3000A-4000A; The first preset ratio value is 0.10 wt %; The first preset pressure value is 0.1 kPa.
2. The method for preparing a low-oxygen rare earth alloy cored wire blank according to claim 1, characterized in that: Before preparing rare earth oxides and rare earth fluorides by molten salt electrolysis, the method also includes: Removing free water and crystal water of electrolyte in the rare earth oxide raw material, the rare earth fluoride, alkali metal and alkaline earth metal fluoride; The cathode and crucible in the electrolysis equipment, the straw, the guide tube, the buffer tank in the negative pressure transfer device and the cored wire blank mold are baked, the baking temperature is a second preset temperature, and the baking time is a second preset duration.
3. The method for preparing a low-oxygen rare earth alloy cored wire blank according to claim 2, characterized in that: The second preset temperature has a numerical range of 200°C-500°C; The numerical range of the second preset time length is 8h-12h.
4. The method for preparing a low-oxygen rare earth alloy cored wire blank according to claim 1, characterized in that: The gas source is an inert gas, and its oxygen content is ≤10ppm; The heating temperature of the heating jacket is 900-1100°C.
5. The method for preparing a low-oxygen rare earth alloy cored wire blank according to claim 4, characterized in that: The sum of the volumes of the buffer tank and the plurality of cored wire blank molds is greater than the sum of the volumes of the negative pressure cavity, the suction pipe, and the guide pipe.
6. The method for preparing a low-oxygen rare earth alloy cored wire blank according to any one of claims 1 to 5, characterized in that: The cored wire blank mold is made of one of pure iron, low carbon steel, stainless steel tube, titanium alloy tube, and nickel alloy tube, and its oxygen content is ≤0.01wt.%; The outer diameter of the cored wire blank die has a numerical range of 20 mm to 50 mm, the wall thickness has a numerical range of 3 mm to 6 mm, and the length has a numerical range of 0.4 m to 1.2 m.
7. The method for preparing a low-oxygen rare earth alloy cored wire blank according to claim 6, characterized in that: The outer diameter of the cored wire blank has a numerical range of 25 mm to 30 mm, and the length of the cored wire blank has a numerical range of 0.5 m to 1 m.
8. The method for preparing a low-oxygen rare earth alloy cored wire blank according to any one of claims 1 to 5, characterized in that: The rare earth in the rare earth alloy liquid accounts for 60 wt.%-98 wt.%, and the rare earth includes one or more of lanthanum, cerium, praseodymium, neodymium, and yttrium; The balance of the rare earth alloy liquid includes one or more of iron, titanium, and cobalt, or the balance of the rare earth alloy includes one or more of aluminum and magnesium.
9. The method for preparing a low-oxygen rare earth alloy cored wire blank according to any one of claims 1 to 5, characterized in that: The relationship coefficient k between the mass of the rare earth oxides and rare earth fluorides input in the molten salt electrolysis preparation process and the mass of the output rare earth products is: k=1.02~1.05, in, , is the mass of the rare earth element in the rare earth oxide, is the mass of the rare earth element in the rare earth fluoride, is the mass of rare earth elements in the rare earth product.
Citation Information
Patent Citations
Preparation method of rare earth-iron intermediate alloy for low-oxygen rare earth steel
CN106756446A
Production method of low-oxygen-content rare earth wire
CN113134596A
Electrolytic bath and method for electrolyzing light rare earth metals or alloys
CN103540961A
Metal discharge device of large rare earth molten salt electrolytic bath
CN107012486A
Short-flow method for preparing low-oxygen high-purity rare earth metal
CN111621815A