Black phosphorus composite material, antibacterial nanofiber material, preparation method and application
The black phosphorus composite material formed by forming a Z-shaped heterojunction of black phosphorus nanosheets and hypoxia tungsten oxide WO3-x, solves the problem of insufficient antibacterial performance of fiber products, and achieves efficient sterilization under light, which is suitable for a variety of antibacterial scenarios.
Patent Information
- Application Number
- CN202211556945.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Due to the porous structure and the chemical structure of polymers, existing fiber products are easily a place for microorganisms to survive and reproduce, resulting in insufficient antibacterial performance, and current fungicides lack broad-spectrum killing effects on bacteria.
The black phosphorus nanosheets are used to form a Z-type heterojunction with hypoxia WO3-x. The black phosphorus nanosheets are coated with acrylate PDDA to adjust its potential data, and mixed with hypoxia WO3-x to form a black phosphorus composite Material, doped in fibers to obtain antibacterial nanofiber material.
Under light, black phosphorus composite materials can efficiently generate ROS through the combined action of photocatalysis and photothermal therapy, significantly improve the antibacterial properties of fibers, and have broad-spectrum bactericidal ability. They are suitable for fabrics such as masks, clothing and filters that frequently contact bacteria such as fabrics with frequent bacterial contact. .
Smart Images

Figure CN116084041B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of modified nanomaterials, and in particular to a black phosphorus composite material, including an antibacterial nanofiber material of the black phosphorus composite material, a preparation method of the material and an application thereof. Background Art
[0002] The harm caused by bacterial infection has a huge impact on the global economy and human health. Several large-scale plague outbreaks and infectious diseases in history are closely related to the spread of pathogens. Therefore, as people's awareness of health protection increases, their requirements for masks (including N95 grade) and clothing are no longer limited to basic needs such as body barriers and body temperature. How to give fibers and fabrics antibacterial properties has become the focus of today's society.
[0003] In people's lives, fibers occupy an increasingly important position due to their large elastic modulus, small plastic deformation, and high strength. Especially in people's clothing, such as clothes and masks, fibers are indispensable. However, fiber products are conducive to the attachment of microorganisms due to their porous structure and the chemical structure of high molecular polymers, making such fiber products a good host for the survival and reproduction of microorganisms, which is harmful to human health. Therefore, how to make fibers have antibacterial properties has become a research focus.
[0004] A simple and effective strategy is to prepare hybrid nanofibers by adding fungicides through physical doping or chemical combination. Currently, fungicides used as dopants mainly include quaternary ammonium compounds, N-halamines, antimicrobial peptides, noble metal nanoparticles and metal oxides. However, these fungicides lack a broad-spectrum killing effect on various bacteria.
[0005] Photosensitizers (PS) have become a major member of antibacterial applications, using the controllability of light, negligible drug resistance, and broad-spectrum antibacterial properties to achieve high efficiency. PS can be used for photothermal therapy (PTT) antibacterial under light, that is, near-infrared (NIR) light is converted by PS into local heat for bacterial inhibition. At the same time, PS can also produce toxic reactive oxygen species (ROS) under light, which can quickly react with a wide spectrum of microorganisms (including Gram-positive and Gram-negative bacteria, fungi, and capsid and lipid membrane viruses), kill bacteria, and significantly reduce the risk of further infection. ROS mainly include singlet oxygen ( 1 O2), superoxide anion radical (·O 2- ) and hydroxyl radicals (·OH), 1 The diffusion distance of O2 in air (2-3.5 mm) is much greater than that in water (300 nm), which makes PS immobilized coatings and textiles produce 1 O2 has the ability to remotely inactivate bacteria and viruses in the air. In addition, OH is considered to be the strongest oxidant for microbial inactivation and pollution degradation. However, so far, most of the1 PS of O2 and ·OH need ultraviolet or blue light to excite, such as TiO2, ZnO and SnWO4. However, ultraviolet or blue light has the disadvantages of mutation induction, low penetration and small proportion of natural environment. 1 PS containing O2 and ·OH have attracted great interest as antimicrobial agents.
[0006] Among the reported materials, black phosphorus nanosheets (BPNs) have attracted great interest due to their unique chemical and physical properties. Based on the many characteristics of BPNs, such as high carrier mobility, tunable optical absorption, and band gaps ranging from 0.3 eV in bulk to 2.0 eV in monolayer, BPNs have been shown to have great potential in light-driven energy conversion processes both theoretically and experimentally. It is worth noting that studies have found that BPNs have a novel electronic band structure that can lead to significantly enhanced self-energy correction and exciton effects and contain subband structures. Such properties enable BPNs to generate ROS in photocatalysis, that is, they can be generated by excitation of visible light and ultraviolet light, respectively. 1 O2 and ·OH. In photocatalysis, a heterojunction is usually constructed to achieve effective separation of holes and electrons and improve photocatalytic performance. Heterojunctions are divided into type I heterojunctions, type II heterojunctions, Z-type heterojunctions, S-type heterojunctions, and other types. In the study of black phosphorus, related heterojunction types have been studied. But in general, the surface and edges of BPNs are easily oxidized by O2 and H2O, resulting in a decrease in crystallinity. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a black phosphorus composite material and an antibacterial nanofiber material including the black phosphorus composite material, and also provides a preparation method and application of the material.
[0008] The present invention provides a black phosphorus composite material, wherein the black phosphorus composite material comprises black phosphorus nanosheets BPNs and oxygen-deficient tungsten oxide WO 3-x The surface of the black phosphorus nanosheet BPNs is coated with acrylate PDDA, and the acrylate PDDA is used to adjust the potential data of the black phosphorus nanosheet BPNs; the black phosphorus nanosheet BPNs and the oxygen-deficient tungsten oxide WO 3-x A heterojunction is formed between them.
[0009] Preferably, the heterojunction is a Z-type heterojunction.
[0010] The black phosphorus composite material provided by the present invention is doped into fibers to obtain excellent antibacterial fibers, which can be used in various antibacterial scenarios.
[0011] The present invention provides a method for preparing the above-mentioned black phosphorus composite material, characterized in that the preparation method comprises the steps of:
[0012] S1, preparing black phosphorus acrylate BPP formed by coating the black phosphorus nanosheets BPNs with the acrylate PDDA;
[0013] S2. Preparation of the oxygen-deficient tungsten oxide WO 3-x ;
[0014] S3, by mixing the black phosphorus acrylate BPP with the oxygen-deficient tungsten oxide WO 3-x Mixing to obtain a black phosphorus composite material BPPW.
[0015] Preferably, the black phosphorus acrylate BPP is prepared by a liquid stripping method.
[0016] Preferably, the liquid stripping method comprises the steps of:
[0017] S11, adding the acrylate PDDA solution into oxygen-free water, and performing ultrasonic dispersion to obtain a first solution;
[0018] S12, dispersing black phosphorus in the first solution to obtain a first suspension;
[0019] S13, ultrasonically treating the first suspension to obtain a second suspension; and ultrasonically dispersing the second suspension in an ice bath to obtain a third suspension;
[0020] S14, centrifugally dispersing the third suspension and collecting the supernatant; centrifugally separating the supernatant to obtain a first precipitate, and resuspending the first precipitate in oxygen-free water to obtain the black phosphorus acrylate BPP.
[0021] Preferably, the preparation of the oxygen-deficient tungsten oxide WO 3-x The steps include:
[0022] S21, dissolving tungsten chloride in n-butanol, dissolving by ultrasonication, the solution changes from yellow to blue, and stirring is continued to obtain a second solution;
[0023] S22, adding the second solution into a polytetrafluoroethylene reactor, reacting at high temperature and then cooling to room temperature to obtain a fourth suspension;
[0024] S23, centrifuging the fourth suspension, discarding the supernatant, and obtaining a second precipitate;
[0025] S24, washing the second precipitate with a first solvent, then washing the second precipitate with a second solvent, and drying to obtain WO 3-x powder.
[0026] Preferably, the step of preparing the black phosphorus composite material BPPW comprises:
[0027] S31, preparing the black phosphorus acrylate BPP prepared in S2 into a fifth suspension; adding WO 3-x , and obtain the sixth suspension;
[0028] S32, centrifuging the sixth suspension, discarding the supernatant to obtain a third precipitate, washing the third precipitate with a first solvent, then washing the third precipitate with a second solvent, and drying to obtain a gray-blue black phosphorus composite material BPPW powder.
[0029] The present invention also provides an antibacterial nanofiber material, which further includes a black phosphorus composite material and thermoplastic polyurethane TPU, and the black phosphorus composite material is the above-mentioned black phosphorus composite material.
[0030] The present invention also provides a method for preparing the above-mentioned antibacterial nanofiber material, the preparation method comprising the steps of:
[0031] S4. Prepare the thermoplastic polyurethane TPU into a spinning solution, add the black phosphorus composite material into the spinning solution, and prepare the antibacterial nanofiber material BPPWT.
[0032] In addition, the present invention also provides applications of the above-mentioned antibacterial nanofiber material, wherein the antibacterial nanofiber material is applied to masks, clothing or filters.
[0033] The antibacterial nanofiber material provided by the present invention has the properties of high elasticity and high hydrophobicity, and the characteristics of simple preparation process, and is expected to be applied to fabrics that frequently come into contact with bacteria, such as masks, clothing, filters, etc.; moreover, under light, the antibacterial nanofiber material exerts an efficient and convenient bactericidal effect through the combination of photocatalysis and photothermal therapy. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic flow chart of the method for preparing the antibacterial nanofiber material in a specific embodiment of the present invention.
[0035] Figure 2 It is a scanning electron microscope image of black phosphorus nanosheets BPNs in a specific embodiment of the present invention.
[0036] Figure 3 It is the X-ray diffraction pattern of black phosphorus and black phosphorus nanosheets BPNs in a specific embodiment of the present invention.
[0037] Figure 4 It is a Raman spectrum diagram of black phosphorus and black phosphorus nanosheets BPNs in a specific embodiment of the present invention.
[0038] Figure 5 It is oxygen-deficient tungsten oxide WO in the specific embodiment of the present invention. 3-x Scanning electron microscope image of .
[0039] Figure 6 It is oxygen-deficient tungsten oxide WO in the specific embodiment of the present invention. 3-x X-ray diffraction pattern of .
[0040] Figure 7 It is oxygen-deficient tungsten oxide WO in the specific embodiment of the present invention. 3-x X-ray photoelectron spectrum of .
[0041] Figure 8 It is the energy spectrum diagram of the black phosphorus composite material BPPW in a specific embodiment of the present invention.
[0042] Fig. 9 3 is a scanning electron microscope image of the TPU fiber in a specific embodiment of the present invention.
[0043] Fig.10 It is a scanning electron microscope image of the antibacterial nanofiber material BPPWT in a specific embodiment of the present invention.
[0044] Fig.11 Graph showing the contact angle of TPU fibers in a specific embodiment of the present invention.
[0045] Fig.12 It is a contact angle diagram of the antibacterial nanofiber material BPPWT in a specific embodiment of the present invention.
[0046] Fig.13 It is a stress-strain curve diagram of the antibacterial nanofiber material BPPWT in a specific embodiment of the present invention.
[0047] Fig.14 It is a fluorescence spectrum diagram of the reaction of TPU fiber and antibacterial nanofiber material BPPWT with TA after visible light irradiation in a specific embodiment of the present invention.
[0048] Fig.15 It is a UV-visible spectrum diagram of the reaction of TPU fiber and antibacterial nanofiber material BPPWT with ABDA after visible light irradiation in a specific embodiment of the present invention.
[0049] Fig.16 It is a plate count diagram of the antibacterial properties of TPU fiber and antibacterial nanofiber material BPPWT under light and dark conditions after visible light irradiation in a specific embodiment of the present invention.
[0050] Fig.17 It is a scanning electron microscope image of the antibacterial properties of TPU fiber and antibacterial nanofiber material BPPWT under light and dark conditions after visible light irradiation in a specific embodiment of the present invention.
[0051] Fig.18It is the survival rate of various bacteria under light and dark conditions of TPU fiber and antibacterial nanofiber material BPPWT after visible light irradiation in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0053] In a specific embodiment, the present invention provides a black phosphorus composite material, wherein the black phosphorus composite material comprises black phosphorus nanosheets BPNs and oxygen-deficient tungsten oxide WO 3-x The surface of the black phosphorus nanosheet BPNs is coated with acrylate PDDA, the black phosphorus nanosheet BPNs and the oxygen-deficient tungsten oxide WO 3-x A heterojunction is formed between them, where x only represents that the tungsten oxide used for compounding is oxygen-deficient tungsten oxide, and the specific value range is not limited. The heterojunction is a Z-type heterojunction. Compared with other heterojunctions, the heterojunction material can have a more negative conduction band and a more positive valence band, can effectively separate electrons and holes, and has a strong redox ability, and can simultaneously generate hydroxyl radicals and singlet oxygen; according to different synthesis conditions, the best performance oxygen-deficient tungsten oxide can be obtained, which can produce the highest ·OH; in a preferred embodiment, by using a mass ratio of 1:10 BPP:WO 3-x The optimal heterojunction structure can produce more OH and 1 O2 has better killing performance against bacteria.
[0054] In a specific embodiment, the addition of acrylate PDDA is mainly used to affect the potential data of black phosphorus nanosheets BPNs. By using different proportions of acrylate PDDA to coat black phosphorus nanosheets BPNs, BPNs can be provided with different potential data, as shown in Table 1. It can be seen from the table that different potential data can be obtained by adding different proportions of PDDA to the same mass of 20 mg of black phosphorus BP, and black phosphorus BP can be further prepared into black phosphorus nanosheets BPNs. Due to the oxygen-deficient tungsten oxide WO 3-x Black phosphorus nanosheets BPNs are negatively charged. In order to make the two better composite, the potential of BPNs can be adjusted by adjusting the addition ratio of acrylate PDDA.
[0055] Table 1 Potential data corresponding to different ratios of PDDA coated BPNs
[0056] Group 1 2 3 BP (mg) 20 20 20 PDDA(uL) 20 40 80 Zeta(mV) 5.9 13.9 17.6
[0057] The black phosphorus composite material provided by the present invention is doped into fibers to obtain excellent antibacterial fibers, which can be used in various antibacterial scenarios.
[0058] The present invention provides a method for preparing the above-mentioned black phosphorus composite material, characterized in that the preparation method comprises the steps of:
[0059] S1. Prepare the black phosphorus acrylate BPP formed by coating the black phosphorus nanosheets BPNs with the acrylate PDDA; specifically, the black phosphorus can be purchased commercially, and then the black phosphorus nanosheets BPNs required by the present invention can be prepared by an existing commonly used preparation method, and the size of the black phosphorus nanosheets BPNs used is less than 400 nm;
[0060] S2. Preparation of the oxygen-deficient tungsten oxide WO 3-x ;
[0061] S3, by mixing the black phosphorus acrylate BPP with the oxygen-deficient tungsten oxide WO 3-x Mixing to obtain a black phosphorus composite material BPPW.
[0062] In a specific embodiment, the black phosphorus acrylate BPP is prepared by a liquid stripping method, and the liquid stripping method comprises the steps of:
[0063] S11, adding the acrylate PDDA solution into oxygen-free water, and dispersing by ultrasonication to obtain a first solution; in a specific embodiment, 40 μL of the PDDA solution can be added into 100 mL of oxygen-free water and dispersed at 200 W ultrasonic power for 10 min to obtain a first solution.
[0064] S12, dispersing black phosphorus in the first solution to obtain a first suspension; the black phosphorus is commercially purchased block black phosphorus, and the first suspension obtained by dispersion is a suspension of block black phosphorus.
[0065] S13, ultrasonically subjecting the first suspension to obtain a second suspension; ultrasonically dispersing the second suspension in an ice bath to obtain a third suspension; in a specific implementation, the suspension of block black phosphorus is ultrasonically treated by an ultrasonic cleaning machine to obtain black phosphorus nanosheets BPNs of 1000 nm or less, and the second suspension is black phosphorus nanosheets BPNs, at which time the yield of black phosphorus nanosheets BPNs is not large; then, the large block black phosphorus is ultrasonically treated by an ultrasonic probe to obtain more small-sized black phosphorus nanosheets BPNs, thereby increasing the yield of black phosphorus nanosheets BPNs, and obtaining a third suspension; specifically, 100 mg of block black phosphorus can be dispersed to obtain the first suspension, and then ultrasonicated at 900 W for 12 h to obtain the second suspension; then, ultrasonically dispersed in an ice bath for 6 h, with a power of 600 W and an on / off cycle of 2 / 2 s, to obtain a third suspension, which is a suspension of black phosphorus nanosheets BPNs.
[0066] S14, centrifugally dispersing the third suspension and collecting the supernatant; centrifugally separating the supernatant to obtain a first precipitate, and resuspending the first precipitate in oxygen-free water to obtain the black phosphorus acrylate BPP.
[0067] In a specific embodiment, the preparation of the oxygen-deficient tungsten oxide WO 3-x The steps include:
[0068] S21, dissolving tungsten chloride in n-butanol, dissolving by ultrasonication, the solution changes from yellow to blue, and stirring is continued to obtain a second solution; in a specific embodiment, n-butanol can be replaced by different reagents such as ethanol, acetic acid or isopropanol, but n-butanol is preferably used.
[0069] S22, adding the second solution into a polytetrafluoroethylene reactor, cooling to room temperature after high temperature reaction, to obtain a fourth suspension; the purchased tungsten chloride (WCl6) is an orange-yellow powder, and the initial dissolution is an orange-yellow solution. When the dissolution continues, alcoholysis occurs to produce soluble tungsten oxychloride or tungsten oxide as a blue solution, and after high temperature and high pressure reaction, oxygen-deficient tungsten oxide crystals are obtained.
[0070] S23, centrifuging the fourth suspension, discarding the supernatant, and obtaining a second precipitate.
[0071] S24, washing the second precipitate with a first solvent, then washing the second precipitate with a second solvent, and drying to obtain WO 3-x Powder; wherein the first solvent is deionized water, ultrapure water, distilled water, etc.; the second solvent is anhydrous ethanol, etc.
[0072] In a specific embodiment, the step of preparing the black phosphorus composite material BPPW comprises:
[0073] S31, preparing the black phosphorus acrylate BPP prepared in S2 into a fifth suspension; adding WO 3-x , and obtain the sixth suspension;
[0074] S32. Centrifuge the sixth suspension, discard the supernatant to obtain a third precipitate, wash the third precipitate with a first solvent, then wash the third precipitate with a second solvent, and dry to obtain a gray-blue black phosphorus composite material BPPW powder; wherein the first solvent is deionized water, ultrapure water, distilled water, etc.; the second solvent is anhydrous ethanol, etc.
[0075] The present invention also provides an antibacterial nanofiber material, which further comprises a black phosphorus composite material and a thermoplastic polyurethane TPU, wherein the black phosphorus composite material is the above-mentioned black phosphorus composite material. In a specific embodiment, the gray-blue black phosphorus composite material BPPW powder obtained by compounding the oxygen-deficient tungsten oxide and the black phosphorus nanosheets is granular and adheres to the thermoplastic polyurethane TPU fiber. Specifically, the mass ratio of black phosphorus nanosheets: oxygen-deficient tungsten oxide: thermoplastic polyurethane TPU is 1:10:200.
[0076] In a specific embodiment of the present invention, a method for preparing the above-mentioned antibacterial nanofiber material is also provided, and the preparation method comprises the steps of:
[0077] S4, preparing the thermoplastic polyurethane TPU into a spinning solution, adding the black phosphorus composite material into the spinning solution, and preparing the antibacterial nanofiber material BPPWT. The preparation method of the black phosphorus composite material includes the steps described above.
[0078] In addition, in a specific embodiment of the present invention, the application of the above-mentioned antibacterial nanofiber material is also provided, and the antibacterial nanofiber material is applied to masks, clothing or filters.
[0079] In a specific embodiment, the entire preparation method of the antibacterial nanofiber material and the applicable application scenarios are more intuitive as follows: Figure 1 as shown in .
[0080] The following is a further detailed description with reference to specific embodiments.
[0081] Example 1
[0082] (1) Preparation of black phosphorus acrylate BPP
[0083] In this example, black phosphorus acrylate BPP was prepared by a liquid exfoliation method.
[0084] Specifically, 40 μL of PDDA solution was added to 100 mL of anaerobic water and dispersed at 200 W ultrasonic power for 10 minutes to obtain a first solution; 100 mg of block black phosphorus was dispersed in the first solution to obtain a first suspension; the first suspension was placed in a beaker and ultrasonicated at 900 W for 12 hours to obtain a second suspension; the second suspension was ultrasonically dispersed in an ice bath for 6 hours, the ultrasonic power was 600 W, and the ultrasonic on / off cycle was 2 / 2s to obtain a third suspension; the third suspension was centrifuged at a speed of 4000 r / m for 15 minutes, the supernatant was collected, and the supernatant was centrifuged at a speed of 11000 r / m for 20 minutes to obtain a first precipitate, and finally the first precipitate was resuspended in anaerobic water to obtain black phosphorus acrylate BPP.
[0085] (2) Characterization of black phosphorus acrylate BPP
[0086] Although the characterization is actually performed on the black phosphorus acrylate BPP prepared in the previous paragraph, since the acrylate PDDA is mainly used to adjust the potential data of the black phosphorus nanosheets BPNs, the actual characterization is still BPNs; the morphology of BPNs is evaluated by scanning electron microscopy (SEM), and the results are as follows Figure 2 As shown in FIG. 1 , the BPNs prepared in this embodiment have an independent lamellar structure with a diameter in the range of 200-500 nm. The crystal structure of the BPNs was evaluated by X-ray diffraction (XRD). Figure 3 As shown, the angles at 16.8°, 34.2°, and 52.3° correspond to the (020), (040), and (060) planes of BPNs, respectively, which are typical layered planes of BPNs.
[0087] Raman spectroscopy confirmed the structural transformation of bulk BP exfoliation to ultrathin BPNs, providing detailed information on molecular vibration and rotation modes. Figure 4 As shown in the figure, the three typical Raman peaks of bulk black phosphorus BP are located at 365 cm -1 An out-of-plane phonon mode A at 1 g and located at 438cm -1 and 466cm -1 Two in-plane phonon modes B 2 g and A 2 g The characteristic Raman peaks are red-shifted by 1.8 cm -1 , 0cm -1 , 1.8cm -1 , which is attributed to the ultrathin thickness of BPNs, indicating that BPNs were successfully synthesized.
[0088] (3) Oxygen-deficient tungsten oxide WO 3-x Preparation
[0089] 500 mg of tungsten chloride (WCl6) was dissolved in 5 mL of n-butanol and stirred at high speed for 5 minutes, then dissolved in 200 W ultrasonic for 10 minutes, the solution turned from yellow to blue, and continued to stir at high speed for 5 minutes to obtain a second solution; the second solution was poured into a polytetrafluoroethylene reactor, placed in an oven at a temperature of 200°C for 24 hours, and cooled to room temperature to obtain a fourth suspension; the fourth suspension was centrifuged at a speed of 11000 r / m for 5 minutes, and the supernatant was discarded to obtain a second precipitate, which was washed 3 times with ultrapure water, and then washed 3 times with anhydrous ethanol, and finally placed in a vacuum oven at a temperature of 60°C to dry overnight to obtain oxygen-deficient tungsten oxide WO 3-x powder.
[0090] (4) Oxygen-deficient tungsten oxide WO 3-x Characterization
[0091] Evaluation of WO by SEM 3-x The surface morphology of nanomaterials is shown in Figure 2. Figure 5 As shown, WO 3-x It is a petal-shaped sphere composed of 300-600nm flakes with a diameter of about 3μm. 3-x The crystal structure of Figure 5 As shown, WO 3-x The crystal structure of triclinic tungsten oxide (JCPDS card PDF#05-0729) is basically maintained. The existence of oxygen vacancies was confirmed by X-ray photoelectron spectroscopy (XPS) analysis of element valence states. The results are as follows Figure 6 As shown, the high-resolution XPS spectrum of W4f shows two main peaks 4f 5 / 2 (37.5eV) and 4f 7 / 2 (35.4eV). The two strong binding energy peaks are at 35.4eV (W 6+ 4f 7 / 2 ) and 37.5eV(W 6+ 4f 5 / 2 ) and two weak signals, about 34.0 eV (W 5+ 4f 7 / 2 ) and 36.4eV(W 5+ 4f 5 / 2 ) is obtained by fitting Figure 7 The XPS spectrum of W 6+ and W 5+ The atomic ratios of can be calculated to be 95.38% and 4.62% respectively. Therefore, the atomic ratio of O / W in the prepared oxygen-deficient tungsten oxide is about 2.99, that is, x=0.01.
[0092] (5) Preparation of black phosphorus composite material BPPW
[0093] The calculated concentration of black phosphorus acrylate BPP aqueous solution was about 100 μg mL -1 , as the fifth suspension; 50 mg WO 3-x Add 50 mL of the fifth suspension and stir for 4 hours to obtain a sixth suspension; centrifuge the sixth suspension at a rotation speed of 11000 r / m for 5 minutes, discard the supernatant to obtain a third precipitate, wash the third precipitate three times with ultrapure water, and finally place it in a vacuum oven at a temperature of 60°C and dry overnight to obtain a gray-blue black phosphorus composite material BPPW powder, remember the black phosphorus composite material prepared in this embodiment.
[0094] (6) Characterization of black phosphorus composite material BPPW
[0095] The element distribution in the black phosphorus composite material BPPW prepared in this embodiment was analyzed by energy dispersive spectroscopy (EDS). The results are as follows: Figure 8 As shown, EDS shows good coexistence of three different elements, including 3-x The W and O elements from , as well as the P element from black phosphorus acrylate BPP, verify the feasibility of the composite method.
[0096] The ability of black phosphorus acrylate BPP and black phosphorus composite material BPPW to generate hydroxyl radicals and singlet oxygen in this embodiment was evaluated by fluorescence spectrometer and UV-visible photometer. The results are as follows: Fig.14 As shown in the figure, it can be seen that under visible light irradiation, WO 3-x The generated hydroxyl radicals react with terephthalic acid (TA) to generate dihydroxybenzoic acid with an emission wavelength of 425 nm. 3-x The amount of hydroxyl radicals produced decreases with the increase of black phosphorus content. Fig.15 It can be seen that under visible light irradiation, the singlet oxygen produced by black phosphorus reacts with 9,10-anthracenediyl-bis(methylene)dimalonic acid (ABDA), and the ultraviolet absorption decreases with the decrease of ABDA content, indicating that the black phosphorus composite material BPPW can produce more singlet oxygen.
[0097] Example 2
[0098] (1) Preparation of antibacterial nanofiber material BPPWT
[0099] Thermoplastic polyurethane TPU particles (MW = 150,000) were placed in a 60 ° C oven and dried for 1 h. 2.5 g was weighed and dissolved in 10 ml of a mixed solvent (dimethylformamide: tetrahydrofuran = 7:3, DMF:THF = 7:3) and stirred vigorously for 6 h to obtain a spinning solution. The spinning solution was heated at a flow rate of 0.2 mL h -1 Under the conditions of 35°C, temperature and receiving distance of 30 cm, TPU fiber was obtained by blow spinning; similarly, according to the same steps, the black phosphorus composite material BPPW prepared in Example 1 was added to the spinning solution to obtain TPU fiber containing BPPW, that is, the antibacterial nanofiber material BPPWT of this embodiment was obtained.
[0100] (2) Characterization of TPU fiber and antibacterial nanofiber material BPPWT
[0101] The surface morphologies of the TPU fibers and the antibacterial nanofiber material BPPWT prepared in this example were evaluated by SEM. The results are as follows: Fig. 9 and Fig.10As shown in the figure, it can be seen that the diameters of TPU fibers and antibacterial nanofiber material BPPWT are both between 500nm and 1000nm. After adding the black phosphorus composite material BPPW, the fiber diameter increases slightly.
[0102] The hydrophobicity of TPU fiber and antibacterial nanofiber material BPPWT was measured by contact angle meter, and the results were as follows: Fig.11 and Fig.12 As shown in the figure, it can be seen that the contact angle of TPU fiber is 121.7°, which is greater than 90°, indicating its good hydrophobicity. After adding black phosphorus composite material BPPW, the contact angle of antibacterial nanofiber material BPPWT is 112.8°, which decreases slightly, but is still higher than 90°, and is still a hydrophobic material.
[0103] The mechanical properties of the corresponding membranes were measured by a universal testing machine. Fig.13 As shown, all tested nanofibers of TPU fibers exhibit linear elastic behavior in the low stress region and plastic deformation at higher stress levels. After the introduction of the black phosphorus composite material BPPW, the stress-strain curve of the antibacterial nanofiber material BPPWT does not change much. The antibacterial nanofiber material BPPWT prepared in this embodiment still has good flexibility. Under the condition of a tensile stress of 3.99MPa, the breaking strain is 565.6%. Compared with the breaking strain of 40.6% of non-woven fabrics and 80% of polylactic acid in existing commonly used spinning materials, the antibacterial nanofiber material BPPWT prepared in this embodiment has excellent elasticity.
[0104] Example 3
[0105] Antibacterial properties of antibacterial nanofiber material BPPWT
[0106] Dilute the freshly prepared bacterial suspension in normal saline to an OD of 600 The TPU fiber prepared in Example 2 and 25 mg of antibacterial nanofiber material BPPWT were placed in 2 mL of bacterial suspension, and then the sample was exposed to simulated sunlight (100 mW cm -2 ) and dark conditions for 2h; the bacterial suspension was diluted in sequence and inoculated on LB agar plates, and photographed after culture at 37°C.
[0107] Under the scanning electron microscope, the collected bacteria were first fixed in a PBS solution containing 2.5% glutaraldehyde at 4°C overnight, and then dehydrated with ethanol / water mixtures with ethanol volumes of 10%, 30%, 50%, 70%, 90%, and 100%, respectively. Finally, the samples were dropped on a silicon wafer, dried naturally, and sprayed with gold before scanning electron microscope analysis.
[0108] The plate counting method was used to analyze the bacterial activity of Escherichia coli (E.coli), multidrug-resistant Escherichia coli (MDR E.coli), Staphylococcus aureus (S.aureus), methicillin-resistant Staphylococcus aureus (MRSA), etc. after exposure to light after the materials were exposed to light. Fig.16 and Fig.18 As shown, the results show that TPU fiber has no antibacterial effect, and TPU fiber added with black phosphorus composite material BPPW has no obvious antibacterial effect under lightless conditions; However, under light conditions, TPU fiber added with black phosphorus composite material BPPW, that is, the antibacterial nanofiber material BPPWT obtained in Example 2 has a significant antibacterial effect, which can achieve an inhibition efficiency of more than 95%.
[0109] in addition, Fig.17 It is a scanning electron microscope image of the antibacterial properties of thermoplastic polyurethane TPU and antibacterial nanofiber material BPPWT under light and dark conditions after visible light irradiation in a specific embodiment of the present invention. It can be clearly seen from the scanning electron microscope that under light conditions, most of the microorganisms in the TPU fiber to which the BPPW composite material is added, that is, the antibacterial nanofiber material BPPWT obtained in Example 2, are destroyed, wherein the arrows point to damaged bacteria, which fully demonstrates that the antibacterial nanofiber material BPPWT prepared by the present invention has good antibacterial properties.
[0110] The antibacterial nanofiber material provided by the present invention has the properties of high elasticity and high hydrophobicity, and the characteristics of simple preparation process, and is expected to be applied to fabrics that frequently come into contact with bacteria, such as masks, clothing, filters, etc.; moreover, under light, the antibacterial nanofiber material exerts an efficient and convenient bactericidal effect through the combination of photocatalysis and photothermal therapy.
[0111] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Those skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.
[0112] The above specific implementations of the present invention do not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A black phosphorus composite material, It is characterized in that The black phosphorus composite material comprises black phosphorus nanosheets BPNs and oxygen-deficient tungsten oxide WO 3-x The surface of the black phosphorus nanosheet BPNs is coated with acrylate PDDA, and the acrylate PDDA is used to adjust the potential data of the black phosphorus nanosheet BPNs; The black phosphorus nanosheets BPNs and the oxygen-deficient tungsten oxide WO 3-x A heterojunction is formed between them; The preparation method of the black phosphorus composite material comprises the steps of: S1, preparing black phosphorus acrylate BPP formed by coating the black phosphorus nanosheets BPNs with the acrylate PDDA; S2. Preparation of the oxygen-deficient tungsten oxide WO 3-x ; S3, by mixing the black phosphorus acrylate BPP with the oxygen-deficient tungsten oxide WO 3-x Mixing to prepare a black phosphorus composite material BPPW; The black phosphorus acrylate BPP is prepared by a liquid stripping method, which comprises the following steps: S11, adding the acrylate PDDA solution into oxygen-free water, and performing ultrasonic dispersion to obtain a first solution; S12, dispersing black phosphorus in the first solution to obtain a first suspension; S13, ultrasonically treating the first suspension to obtain a second suspension; Ultrasonic dispersion of the second suspension in an ice bath to obtain a third suspension; S14, centrifugally dispersing the third suspension and collecting the supernatant; centrifugally separating the supernatant to obtain a first precipitate, and resuspending the first precipitate in oxygen-free water to obtain the black phosphorus acrylate BPP; The preparation of the oxygen-deficient tungsten oxide WO 3-x The steps include: S21, dissolving tungsten chloride in n-butanol, dissolving by ultrasonication, the solution changes from yellow to blue, and stirring is continued to obtain a second solution; S22, adding the second solution into a polytetrafluoroethylene reactor, reacting at high temperature and then cooling to room temperature to obtain a fourth suspension; S23, centrifuging the fourth suspension, discarding the supernatant, and obtaining a second precipitate; S24, washing the second precipitate with a first solvent, then washing the second precipitate with a second solvent, and drying to obtain WO 3-x powder; The steps of preparing the black phosphorus composite material BPPW include: S31, preparing the black phosphorus acrylate BPP prepared in S2 into a fifth suspension; adding WO 3-x , and obtain the sixth suspension; S32, centrifuging the sixth suspension, discarding the supernatant to obtain a third precipitate, washing the third precipitate with a first solvent, then washing the third precipitate with a second solvent, and drying to obtain a gray-blue black phosphorus composite material BPPW powder.
2. The black phosphorus composite material according to claim 1, It is characterized in that The heterojunction is a Z-type heterojunction.
3. An antibacterial nanofiber material, It is characterized in that The antibacterial nanofiber material also includes a black phosphorus composite material and thermoplastic polyurethane TPU, and the black phosphorus composite material is the black phosphorus composite material according to claim 1 or 2.
4. A method for preparing the antibacterial nanofiber material as claimed in claim 3, It is characterized in that The preparation method comprises the steps of: S4. Prepare the thermoplastic polyurethane TPU as a spinning solution, add the black phosphorus composite material according to claim 1 or 2 into the spinning solution, and obtain the antibacterial nanofiber material BPPWT.
5. An application of the antibacterial nanofiber material as claimed in claim 3, It is characterized in that The antibacterial nanofiber material is applied to masks, clothing or filters.