A ductile iron pipe anticorrosion coating and a method for preparing the anticorrosion coating using the same

By adding specific compositions to cement-based anticorrosion coatings, the composition of the mortar layer is optimized, and the problems of poor pumping properties and insufficient anticorrosion performance are solved, and more efficient anticorrosion coating applications are achieved, extending service life and improving production efficiency .

CN116102315BActive Publication Date: 2024-11-15XINXING DUCTILE IRON PIPES CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310062635.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-15
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The existing cement-based anti-corrosion coatings have poor pumping properties, easy to cause sags, poor anti-corrosion and anti-permeability, and long maintenance cycle, resulting in low service life and production efficiency of ductile iron pipes.

Method used

By adding bentonite and magnesium aluminum silicate to the mortar layer thixotropic lubricants, polycarboxylic acid high-efficiency water reducing agent, emulsion, waterproofing agent, defoaming agent and retarder to the mortar layer, the spraying system of fiber cement mortar is optimized and improved Pumping and corrosion resistance, reducing porosity, enhancing sag resistance and durability.

Benefits of technology

It significantly improves the pumpability and construction properties of the anti-corrosion coating, extends the service life, reduces the maintenance cycle, improves the anti-corrosion effect and production efficiency, and reduces the overall cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The present invention relates to the field of coating materials, and specifically discloses an anti-corrosion coating for a ductile iron pipe and a method for preparing the anti-corrosion coating using the same. The anti-corrosion coating includes a connecting layer and a mortar layer. The connecting layer is an epoxy resin coating or a glass fiber mesh cloth layer; the raw materials of the mortar layer include the following components by mass: the raw materials of the mortar layer include 80 to 120 parts of cement, 80 to 200 parts of sand, 0.05 to 0.5 parts of thickening dispersant, 0.5 to 2 parts of fiber, 0.1 to 3 parts of water reducer, 0.1 to 2.5 parts of thixotropic lubricant and 20 to 40 parts of water. Through the synergistic effect of each component, the anti-corrosion coating has excellent properties such as resistance to chemical erosion, permeability resistance, durability, acid and alkali resistance, etc. The preparation method of the anti-corrosion coating is simple, the production efficiency is high, the coating life is long, the cost is low, and it meets the production and use requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipeline cement coatings, and in particular provides an anti-corrosion coating for a ductile iron pipe and a method for preparing the anti-corrosion coating by using the same. Background Art

[0002] Ductile iron pipes have been used in underground and overhead environments for hundreds of years and are widely used in water conservancy, water supply, drainage and other fields. At present, when such pipelines are used in overhead and buried environments, organic anti-corrosion coatings are widely used. During the transportation, installation and storage of pipelines, if the coating is damaged and not repaired in time, local corrosion will occur, causing corrosion perforation, which seriously reduces the service life and safety of the pipeline. In addition to the standardization of the installation and transportation process, the quality of the anti-corrosion performance is also greatly related to the type and thickness of the anti-corrosion coating. For example, ensuring the long life of the pipeline will lead to an extreme increase in the cost of the product. In addition, when the pipeline is used in a trenchless dragging construction environment, especially in the corrosive and gravel cavity crossing process, the long-distance dragging causes the coating to rub against the hard objects in the soil, causing the pipeline anti-corrosion layer to leak or the anti-corrosion layer to fall off and cannot be found. The pipeline is buried for a long time and is subject to local corrosion or even perforation, causing pipeline leakage.

[0003] In addition to the above, cement-based anti-corrosion coating ductile iron pipe products have appeared on the market in recent years, but there are still major problems. The main problems are as follows; First: The cement-based anti-corrosion coating in the prior art introduces cellulose to increase the consistency and dispersion uniformity, but it is easy to cause poor mortar pumping, resulting in equipment pump blockage, gun blockage and other problems, causing material waste, while reducing production efficiency, and the increase in viscosity leads to an increase in pores in the mortar layer, reduced strength, poor appearance quality, and easy to cause problems such as sagging. Second: The mortar layer shrinks and deforms under the temperature rise changes in its later maintenance, resulting in many tiny cracks inside it. Under the influence of the external environment, these cracks will further develop and extend, especially under the erosion of infiltrating water flow, the concrete may form concentrated or penetrating water seepage channels due to excessive crack development, and ultimately lead to overall destruction of the concrete structure. Due to the poor waterproof performance of concrete itself, the durability of the pipe is reduced, so it is inevitable to take reasonable measures to improve the anti-seepage performance and mechanical properties of the mortar layer. Third: In the prior art, the bonding between the connecting layer and the mortar layer is complicated, which increases the difficulty of outputting finished products and easily generates gaps, resulting in a greater risk of coating peeling in the later stage.

[0004] In summary, the existing technology of cement-based anti-corrosion coating for ductile iron pipes still has problems such as complex process, high cost, poor performance of some anti-corrosion coatings, low production efficiency, etc., which makes it inconvenient to apply them in production and life. Therefore, the invention of a cement-based anti-corrosion coating for ductile iron pipes with excellent performance is of great significance for both industrial production and daily life. Summary of the invention

[0005] In view of the technical problems in the above-mentioned prior art that cement-based anti-corrosion coating materials have poor pumpability, are prone to sagging, have poor anti-corrosion and anti-permeability properties, and have a long maintenance period, the present invention provides an excellent ductile iron pipe anti-corrosion coating and a preparation method thereof, which improves the pumping performance of the mortar mixture while improving its anti-sagging performance and service life, reduces the proportion and size of bubbles in the coating, improves its anti-corrosion, anti-permeability and fracture resistance, optimizes the spraying system of the fiber cement mortar, reduces the maintenance period and improves production efficiency.

[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0007] A first aspect of the present invention provides an anti-corrosion coating for a ductile iron pipe, the anti-corrosion coating comprising a connecting layer and a mortar layer;

[0008] The raw materials of the mortar layer include the following components in parts by mass: the raw materials of the mortar layer include 80 to 120 parts of cement, 80 to 200 parts of sand, 0.05 to 0.5 parts of thickening dispersant, 0.5 to 2 parts of fiber, 0.1 to 3 parts of water reducing agent, 0.1 to 2.5 parts of thixotropic lubricant and 20 to 40 parts of water;

[0009] Preferably, the thixotropic lubricant is bentonite and magnesium aluminum silicate in a mass ratio of 1:1-1.5.

[0010] Preferably, the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0011] More preferably, the water reducer is polycarboxylic acid high-efficiency water reducer powder.

[0012] Compared with the prior art, the present invention prepares a new type of anticorrosive coating material by combining a connecting layer and a mortar layer. By adding a series of raw material compositions and combining and compounding them, the pumpability and workability of the cement-based anticorrosive coating are effectively improved, the porosity of the anticorrosive coating is reduced, and the anticorrosive life and anticorrosive effect of the anticorrosive coating are improved. Among them, the thixotropic lubricant composited by bentonite and magnesium aluminum silicate can be used as a stabilizer for the mortar, which can effectively maintain the consistency stability of the mortar system, and also has a certain hydrophilicity that can better improve the performance of the suspension system, and can also improve the anti-sagging and storage stability of the coating material, and overcome the negative effects of mortar sagging or agglomeration during construction. In addition, the thixotropic lubricant can also improve the construction pumpability and shear thinning, reduce the friction between cement and sand particles, have a slippery effect, make the mortar easy to pump, make pumping more convenient, improve the transportation efficiency, thereby reducing the overall cost and reducing construction losses. Since polycarboxylic acid water-reducing agent has good compatibility with cement, and polycarboxylic acid high-efficiency water-reducing agent powder as mortar does not contain water, the added amount is small, the water-reducing effect is better, and it can greatly improve the early and late strength of concrete. In addition, the chloride ion content is low, which is more conducive to the durability of the coating. The addition of water-reducing agent can greatly reduce the water demand of the mortar layer and avoid serious shrinkage cracks caused by subsequent water loss.

[0013] Preferably, the mortar layer raw materials further include 1 to 20 parts of emulsion.

[0014] Preferably, the emulsion is one or both of styrene-butadiene polymer emulsion and styrene-acrylate polymer emulsion.

[0015] More preferably, the emulsion is a styrene acrylic emulsion.

[0016] Styrene acrylic emulsion can effectively fill pores, reduce the shrinkage rate of modified mortar, improve its density, and form a polymer layer at the interface between cement paste and aggregate and unhydrated cement particles, which improves the interfacial bonding between hydration products and aggregate and unhydrated cement particles and improves the flexural strength. In addition, styrene acrylic emulsion is compatible with cement and can react chemically with the cement matrix to a certain extent, enhancing the bonding between the polymer film and the cement matrix, which can significantly improve the mechanical strength and water resistance of the mortar. The microstructure of the polymer-modified cement-based material is improved under the combined action of chemical reaction and physical wrapping. The complete network structure formed by the polymer film, as the cement is hydrated, the generated hydration products are interspersed in the polymer film, and finally form an interwoven organic-inorganic interpenetrating structure, thereby improving the microstructure of the cement-based material. At the same time, the hydrophilic colloidal properties of the emulsion and the filling and sealing effects of the formed polymer film on the connected capillaries are used to prevent the loss of water in the cement paste. Therefore, the water required for cement hydration is retained in the cement mortar matrix to make it more fully hydrated. At the same time, this has a certain improvement effect on the bonding strength and self-strength development of the mortar constructed on a highly absorbent matrix. In addition, with the increase in the amount of emulsion, the volume density decreases. The decrease in the volume density of the modified cement mortar is due to the introduction of a large number of bubbles by the addition of the polymer, which increases the air content in the modified cement mortar. This is mainly attributed to the "ball" effect of the air introduced by the polymer particles and the dispersing effect of the polymer particles adsorbed on the surface of the cement particles, thereby improving the working performance of the cement mortar. The appropriate proportion of emulsion can increase the flowability of the modified cement mortar to the point where the bubbles in the mortar system can be smoothly removed, reducing the air content in the mortar layer.

[0017] Preferably, the mortar layer raw materials also include 0.2 to 5 parts of a waterproofing agent.

[0018] Preferably, the waterproofing agent is a silicone waterproofing agent.

[0019] More preferably, the waterproofing agent is sodium methyl silicate.

[0020] The addition of waterproofing agent can not only form a water-blocking layer on the surface of concrete through penetration crystallization, but also can use the penetration water pressure to penetrate into the pore channels in the mortar layer, and produce complex crystallization reaction through the active materials in its own components and the moisture and free active ingredients in the mortar layer, forming an insoluble crystal complex that blocks the internal capillary channels and tiny cracks, thereby improving the density, durability and impermeability of the mortar layer. In addition, waterproofing agent can react chemically with calcium hydroxide, aluminum hydroxide, metal oxides and salt substances in cement mortar to form insoluble crystals. These crystalline structures can block and fill tiny cracks, holes and pores. When the mortar layer is dry, it is in a dormant state. Once it comes into contact with water, it will be activated to form new crystals again, fill and block new leakage defects, and provide a permanent self-repair function for the mortar layer. At the same time, the addition of waterproofing agent can improve the freeze-thaw resistance and acid corrosion resistance of the coating material.

[0021] Preferably, the mortar layer raw materials further include 0.05 to 0.5 parts of a defoaming agent.

[0022] Preferably, the defoamer is at least one of a silicone defoamer, a polyether defoamer, a high-carbon alcohol defoamer, a mineral oil defoamer or a vegetable oil defoamer.

[0023] More preferably, the defoaming agent is a silicon defoaming agent.

[0024] The defoamer can make the cement-based anticorrosive coating raw material composition form uniform and stable small bubbles, improve the workability of the mortar, and enhance the density of the mortar. The addition of the defoamer can well solve the problem of high viscosity and many internal pores in the mortar layer system, reduce the local pores in the mortar layer, and improve the overall density and strength. The defoamer plays an important role in enhancing exhaust in the process of spraying mortar.

[0025] Preferably, the mortar layer raw materials further include 0.1 to 3 parts of a retarder.

[0026] Preferably, the retarder is one or more of tartaric acid, sodium gluconate or boric acid.

[0027] Retarder can delay the setting time of fiber cement mortar, prevent the mixture from setting too quickly in the initial stage of pumping and during the pumping process, and keep the construction going smoothly.

[0028] Preferably, the connecting layer comprises one of an epoxy resin coating or a glass fiber mesh cloth layer;

[0029] Preferably, the epoxy resin coating is a water-based epoxy resin.

[0030] Preferably, the glass fiber mesh cloth is a self-adhesive mesh cloth with a mesh size of 2 to 4 mm.

[0031] Water-based epoxy resin can easily penetrate into the surface of the mortar layer and form stable adhesion performance by cross-linking with the mortar layer. The self-adhesive mesh can be bonded to the pipe and fit tightly to avoid leaving large gaps. The mesh is easy to embed in the mortar and provides better adhesion performance.

[0032] Preferably, the cement is general purpose Portland cement.

[0033] More preferably, the strength grade of the silicate cement is one of 42.5, 42.5R, 52.5 or 52.5R.

[0034] Generally, cement with strength grade of 42.5 is selected to keep product cost low and the strength meets the requirements of on-site construction.

[0035] Preferably, the sand is natural sand or machine-made sand.

[0036] More preferably, the sand is natural sand.

[0037] Preferably, the sand particle size is not less than 4 mesh.

[0038] More preferably, the sand particle size is 8 mesh to 100 mesh.

[0039] Natural sand weathers into rounded corners in the natural environment, which is more conducive to pumping and reduces damage to the screw pump. The mesh size of the sand affects the pumping effect and the strength of the mortar layer. Sand particles with 8-100 meshes tend to reduce the internal pores of the mortar to improve the strength of the mortar layer. Sand with a lower mesh size is more conducive to pumping, but it will affect the strength of the mortar layer.

[0040] Preferably, the fiber is one of polypropylene fiber or glass fiber.

[0041] More preferably, the polypropylene fiber can be selected from polypropylene mesh fiber or polypropylene monofilament fiber.

[0042] The glass fiber is one of alkali-resistant glass fiber and alkali-resistant glass fiber.

[0043] More preferably, the polypropylene fiber is a polypropylene mesh fiber.

[0044] Preferably, the fiber length is 6 to 9 mm.

[0045] Polypropylene fiber has a better effect in solving the problem of fiber agglomeration and poor dispersion, while glass fiber can avoid reducing the service life of the mortar layer due to the alkaline effect of the mortar layer.

[0046] Preferably, the thickening and dispersing agent is cellulose.

[0047] More preferably, the thickening and dispersing agent is hydroxypropyl methylcellulose.

[0048] Preferably, the viscosity of the thickening dispersant is 50,000 mPa.s to 200,000 mPa.s.

[0049] More preferably, the usage amount needs to be adjusted according to the viscosity type of the selected cellulose, and the usage amount of high-viscosity cellulose will generally be reduced accordingly.

[0050] Thickening dispersant (hydroxypropyl methylcellulose (HPMC)) is a long-chain polymer that can change the rheological properties of the solution and make the solution have a lower Reynolds number, thereby greatly reducing the degree of freedom of the fiber in the water and reducing the agglomeration phenomenon caused by contact and collision between fibers. In addition, after the dispersant solution is adsorbed on the fiber surface, it helps to reduce the entanglement phenomenon caused by friction between fibers and has a certain water retention effect. However, the addition of thickening dispersant will increase the viscosity of the fiber cement mortar mixture. At the same time, the addition of dispersant reduces the surface tension of the solution and affects the mechanical properties of the fiber cement mortar. The addition of hydroxypropyl methylcellulose and a certain amount of thixotropic lubricant have a synergistic thickening effect and can better improve the performance of the suspension system. In addition, the thickening dispersant can form hydrogen bonds with cellulose to synergistically increase the viscosity of the mortar system, so that the distribution of various components in the grouting slurry remains uniform, prevent the sinking of aggregates, make the slurry homogeneous and stable, and prevent the slurry from settling, stratification and water seepage, thereby improving the water retention performance of the system.

[0051] A second aspect of the present invention provides a method for preparing an anti-corrosion coating for a ductile iron pipe, comprising at least the following steps:

[0052] S1: Weighing each component according to the designed ratio, mixing the solid material and the liquid material respectively to prepare a solid mixed material and a liquid mixed material, and then mixing the solid mixed material and the liquid mixed material to obtain a mortar layer raw material mixture;

[0053] S2: preparing a connection layer on the outer surface of the ductile iron pipe;

[0054] S3: spraying the mortar layer raw material mixture onto the connection layer surface of the ductile iron pipe respectively, grinding and curing, and obtaining the ductile iron pipe anti-corrosion coating.

[0055] Preferably, the polishing is performed by mechanically polishing the sprayed mortar layer using a HMP-150 polishing machine.

[0056] Preferably, the curing is performed at room temperature or by steam so that the mortar layer is completely hydrated.

[0057] The normal temperature health care refers to natural health care for 4-30 hours.

[0058] The steam curing is the curing in a curing chamber at 30° C.-60° C. and relative humidity above 90% for 4-20 hours in a closed manner.

[0059] Preferably, in S1, if the raw materials of the mortar layer include only basic components, the solid mixed material is a material obtained by mixing cement, sand, thickening dispersant, water reducing agent, thixotropic lubricant and fiber, and the liquid mixed material is water; if the raw materials of the mortar layer also include a retarder or a waterproofing agent, the solid mixed material is a material obtained by mixing the retarder or the waterproofing agent with basic components other than water, and the liquid material is water; if the raw materials of the mortar layer also include an emulsion or a defoaming agent, the liquid mixed material is a material obtained by mixing the emulsion or the defoaming agent with water.

[0060] Preferably, in S3, the quick-setting agent and the mortar layer raw material mixture can also be sprayed onto the surface of the connecting layer of the ductile iron pipe, polished and cured to obtain the ductile iron pipe anti-corrosion coating.

[0061] Preferably, the accelerating setting agent is one or more of an alkaline earth metal carbonate accelerating setting agent, a composite sulphoaluminate accelerating setting agent or an aluminate accelerating setting agent.

[0062] More preferably, the accelerating setting agent is alkaline earth metal carbonate.

[0063] Further preferably, the accelerating setting agent is a TR-SN accelerating setting agent.

[0064] The accelerator is output by a separate pump body, and the accelerator is continuously injected into the discharge port of the raw material composition so that the accelerator is evenly mixed with the raw material composition and simultaneously coated on the outer wall of the pipe. The accelerator provides an alkaline environment for the system, causing the gypsum in the cement slurry to transform into Na2SO4, and C3A to rapidly hydrate into ettringite, thereby accelerating the coagulation of the cement slurry. The formation of ettringite also causes a decrease in the concentration of liquid Ca(OH)2, which promotes the hydration of C3S and further accelerates the coagulation of cement. In addition, fine needle-shaped ettringite can be generated to cause the cement to set quickly. The generation of fine needle-shaped ettringite causes the cement to set quickly. Al2(SO4)3 and CaSO4 in cement provide a large amount of SO4 2- , reacts rapidly with Al2O3, Ca(OH)2, etc. in the liquid phase to generate fine needle-shaped ettringite and intermediate product secondary gypsum. These new crystals grow and distribute between cement particles, cross-linking into a network structure, which leads to rapid setting of cement slurry. At the same time, the formation of ettringite reduces the concentration of Ca(OH)2 in the liquid phase, promoting the hydration of silicate components, especially C3S.

[0065] Preferably, after curing in S3, the step of coating the infiltration crystallization agent on the surface of the ductile iron pipe is also included.

[0066] Preferably, the penetrating crystallization agent is Pengneichuan concrete protective agent (PNC701).

[0067] Preferably, the mass fraction of the osmotic crystallization agent is 0.1-1 part.

[0068] The penetrating crystallizer can penetrate into the mortar layer to form a waterproof and protective barrier of a certain depth. In addition, the penetrating crystallizer can also react with the mortar layer to form a gel to seal the holes, capillaries and cracks in the mortar. Once it encounters water, it can continue to seal the fine cracks caused by thermal expansion and contraction.

[0069] The present invention provides an anti-corrosion coating for a ductile iron pipe and a preparation method thereof. By compounding various materials of a mortar layer of the anti-corrosion coating, good pumpability and workability are achieved, and the porosity of the anti-corrosion coating is reduced, thereby increasing the anti-corrosion life and anti-corrosion effect of the anti-corrosion coating. The coating has excellent stability, anti-sagging performance, corrosion resistance, durability, etc. The preparation method is simple, reduces process operation costs, increases the service life of the mortar layer, and improves product production efficiency and quality.

[0070] The following is a further description of a pipeline cement-based anti-corrosion coating raw material composition and a preparation method thereof of the present invention. DETAILED DESCRIPTION

[0071] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0072] The sources of raw materials in Examples 1-3 are as follows:

[0073] 1. Cement: ordinary Portland cement (42.5 cement);

[0074] 2. Sand: river sand and use a 2mm filter to filter out sand with a particle size of more than 2mm;

[0075] 3. Pipe: finished pipe with zinc coating;

[0076] 4. Fiber: polypropylene mesh fiber;

[0077] 5. Thickening and dispersing agent: Hydroxypropyl methylcellulose, Brookfield viscosity 200,000 mPa.s;

[0078] 6. Thixotropic lubricant: bentonite and magnesium aluminum silicate in a mass ratio of 1:1-1.5;

[0079] 7. Emulsion: Styrene acrylic emulsion ( PS 608ap);

[0080] 8. Water reducing agent: polycarboxylic acid high efficiency water reducing agent (powder) 4930F;

[0081] 9. Retarder: tartaric acid;

[0082] 10. Defoaming agent: silicone defoaming agent;

[0083] 11. Waterproofing agent: Concrete waterproofing additive (PNC803);

[0084] 12. Accelerator: TR-SN type accelerator;

[0085] 13. Penetration crystallization agent: Concrete protective agent (PNC701).

[0086] Example 1

[0087] The present embodiment provides a cement-based anti-corrosion coating comprising: 100 parts of Portland cement, 160 parts of sand, 0.8 parts of fiber, 0.3 parts of water reducer, 0.1 parts of thickening dispersant, 0.8 parts of retarder, 0.1 parts of defoaming agent, 0.8 parts of waterproofing agent, 0.2 parts of thixotropic lubricant and 35 parts of water.

[0088] The method for preparing the anticorrosive coating of ductile iron pipe comprises the following steps:

[0089] S1: Weigh each component according to the above ratio, mix and stir the weighed cement, sand, thickening dispersant, thixotropic lubricant, water reducing agent, retarder and fiber for 3 minutes to obtain a solid mixture;

[0090] Weigh each component according to the above ratio, mix and stir the weighed water and defoamer for 2 minutes to obtain a liquid mixture;

[0091] The solid mixture and the liquid mixture are mixed and stirred for 3 minutes to obtain a mortar layer raw material mixture;

[0092] S2: Wrap and bond a glass fiber mesh cloth with a mesh size of 2 to 4 mm to the outer surface of the ductile iron pipe and compact it;

[0093] S3: Evenly mix the raw material mixture of the mortar layer at the nozzle of the spray gun, spray it onto the surface of the connecting layer of the ductile iron pipe, grind it mechanically, cure it at room temperature for 24 hours, clean the surface dust, and apply 0.3 parts of the penetrating crystallization agent to the surface of the ductile iron pipe to obtain the anti-corrosion coating of the ductile iron pipe.

[0094] Example 2

[0095] The present embodiment provides a cement-based anti-corrosion coating, including: 100 parts of aluminate cement, 180 parts of sand, 15 parts of accelerator, 15 parts of emulsion, 1.2 parts of fiber, 0.4 parts of water reducer, 0.4 parts of thickening dispersant, 0.3 parts of retarder, 0.2 parts of defoamer, 1.0 parts of waterproofing agent, 0.2 parts of thixotropic lubricant and 40 parts of water.

[0096] The method for preparing the anti-corrosion coating of ductile iron pipe comprises the following steps:

[0097] S1: Weigh each component according to the above ratio, mix and stir the weighed cement, sand, thickening dispersant, thixotropic lubricant, water reducer, retarder, fiber and waterproofing agent for 3 minutes to obtain a solid mixture;

[0098] Weigh each component according to the above ratio, mix and stir the weighed water, emulsion and defoamer for 2 minutes to obtain a liquid mixture;

[0099] The solid mixture and the liquid mixture are mixed and stirred for 3 minutes to obtain a mortar layer raw material mixture;

[0100] S2: Wrap and bond a glass fiber mesh cloth with a mesh size of 2 to 4 mm to the outer surface of the ductile iron pipe and compact it;

[0101] S3: Place the accelerator in the accelerator pump and connect it to the cement mortar spray gun, turn on the cement mortar spray pump and the accelerator pump, mix the mortar layer raw material mixture evenly at the spray gun nozzle, and spray it onto the connecting layer surface of the ductile iron pipe, grind it mechanically, and cure it at room temperature for 24 hours, then clean the surface dust, apply 0.5 parts of penetrating crystallization agent to the surface of the ductile iron pipe to obtain the ductile iron pipe anti-corrosion coating.

[0102] Example 3

[0103] The present embodiment provides a cement-based anti-corrosion coating, comprising: 100 parts of Portland cement, 180 parts of sand, 15 parts of accelerator, 10 parts of emulsion, 1.2 parts of fiber, 0.5 parts of thickening dispersant, 1.0 parts of waterproofing agent, 0.1 parts of thixotropic lubricant and 45 parts of water.

[0104] The method for preparing the anti-corrosion coating of ductile iron pipe comprises the following steps:

[0105] S1: Weigh each component according to the above ratio, mix and stir the weighed cement, sand, thickening dispersant, thixotropic lubricant, fiber and waterproofing agent for 3 minutes to obtain a solid mixture;

[0106] Weigh each component according to the above ratio, mix and stir the weighed water and emulsion for 2 minutes to obtain a liquid mixture;

[0107] The solid mixture and the liquid mixture are mixed and stirred for 3 minutes to obtain a mortar layer raw material mixture;

[0108] S2: Wrap and bond a glass fiber mesh cloth with a mesh size of 2 to 4 mm to the outer surface of the ductile iron pipe and compact it;

[0109] S3: Place the accelerator in the accelerator pump and connect it to the cement mortar spray gun, turn on the cement mortar spray pump and the accelerator pump, mix the mortar layer raw material mixture evenly at the spray gun nozzle, and spray it onto the connecting layer surface of the ductile iron pipe, grind it mechanically, and cure it at room temperature for 24 hours, then clean the surface dust, apply 0.3 parts of penetrating crystallization agent to the surface of the ductile iron pipe to obtain the ductile iron pipe anti-corrosion coating.

[0110] Example 4

[0111] The present embodiment provides a cement-based anti-corrosion coating, comprising: 100 parts of Portland cement, 180 parts of sand, 15 parts of accelerator, 1.2 parts of fiber, 0.5 parts of thickening dispersant, 0.3 parts of retarder, 0.2 parts of defoamer, 0.1 parts of thixotropic lubricant and 45 parts of water.

[0112] The method for preparing the anti-corrosion coating of ductile iron pipe comprises the following steps:

[0113] S1: Weigh each component according to the above ratio, mix and stir the weighed cement, sand, thickening dispersant, thixotropic lubricant, retarder and fiber for 3 minutes to obtain a solid mixture;

[0114] Weigh each component according to the above ratio, mix and stir the weighed water and defoamer for 2 minutes to obtain a liquid mixture;

[0115] The solid mixture and the liquid mixture are mixed and stirred for 3 minutes to obtain a mortar layer raw material mixture;

[0116] S2: Wrap and bond a glass fiber mesh cloth with a mesh size of 2 to 4 mm to the outer surface of the ductile iron pipe and compact it;

[0117] S3: Place the accelerator in the accelerator pump and connect it to the cement mortar spray gun, turn on the cement mortar spray pump and the accelerator pump, mix the mortar layer raw material mixture evenly at the spray gun nozzle, and spray it onto the connecting layer surface of the ductile iron pipe, grind it mechanically, and cure it at room temperature for 24 hours, then clean the surface dust, apply 0.3 parts of penetrating crystallization agent to the surface of the ductile iron pipe to obtain the ductile iron pipe anti-corrosion coating.

[0118] Comparative Example 1

[0119] This comparative example provides a cement-based anti-corrosion coating, whose formula composition is exactly the same as that of Example 2, except that the bentonite and magnesium aluminum silicate (thixotropic lubricant) in a mass ratio of 1:1-1.5 in Example 2 are replaced with an equal amount of polyamide wax, and the other components and preparation method are the same as those in Example 2 to obtain an anti-corrosion coating for ductile iron pipes.

[0120] Comparative Example 2

[0121] This comparative example provides a cement-based anti-corrosion coating, whose formula composition is exactly the same as that of Example 2, except that the polycarboxylic acid high-efficiency water reducer in Example 2 is replaced with an equal amount of naphthalene-based high-efficiency water reducer, and the other components and preparation method are the same as those of Example 2 to obtain a ductile iron pipe anti-corrosion coating.

[0122] After curing for 30 days, the anti-corrosion coatings of the ductile iron pipes prepared in Examples 1-4 and Comparative Examples 1-5 were subjected to adhesion tests according to the GB1720-2020 circle test method, and the test data were analyzed. The specific results are shown in Table 1.

[0123] Table 1 Adhesion test data

[0124]

[0125] In addition, the present invention also conducted anti-sagging performance and impact resistance tests. The anti-sagging performance test standard was tested according to the method of GB / T 9264-2012, and the impact resistance test was tested according to the method of GB / T 1732-1993. The specific test results are shown in Table 2 below.

[0126] Table 2 Anti-sagging performance and impact resistance test data

[0127] Serial number Anti-sagging (μm) Impact resistance(J) Example 1 1250 100J no cracking Example 2 1200 100J no cracking Example 3 1250 100J no cracking Example 4 1020 100J no cracking Comparative Example 1 720 100J severe cracking Comparative Example 2 720 100J slight cracking

[0128] From the data analysis of Table 1 and Table 2, it can be seen that the ductile iron pipe anti-corrosion coating provided by Examples 1-4 of the present invention has excellent adhesion, high anti-sagging and good impact resistance, as well as excellent anti-corrosion, anti-penetration, fracture strength and other properties, optimizes the spraying system of fiber cement mortar, reduces the maintenance cycle and improves production efficiency to meet production needs.

[0129] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A ductile iron pipe anticorrosion coating, characterized in that: The anti-corrosion coating comprises a connecting layer and a mortar layer; The raw materials of the mortar layer include the following basic components in parts by mass: 80-120 parts of cement, 80-200 parts of sand, 0.05-0.5 parts of thickening dispersant, 0.5-2 parts of fiber, 0.1-3 parts of water reducer, 0.1-2.5 parts of thixotropic lubricant and 20-40 parts of water; Wherein, the thixotropic lubricant is bentonite and magnesium aluminum silicate in a mass ratio of 1:1-1.5; The water reducer is a polycarboxylic acid high-efficiency water reducer; The connecting layer includes one of an epoxy resin coating or a glass fiber mesh cloth layer.

2. The anticorrosive coating for ductile iron pipe according to claim 1, characterized in that: The raw materials of the mortar layer also include 1 to 20 parts of emulsion.

3. The anticorrosive coating for ductile iron pipe according to claim 2, characterized in that: The emulsion is one or both of styrene-butadiene polymer emulsion and styrene-acrylate polymer emulsion.

4. The anticorrosive coating for ductile iron pipe according to claim 1, characterized in that: The raw materials of the mortar layer also include 0.2 to 5 parts of waterproofing agent.

5. The anticorrosive coating for ductile iron pipe according to claim 4, characterized in that: The waterproofing agent is a silicone waterproofing agent.

6. The anticorrosive coating for ductile iron pipe according to claim 1, characterized in that: The raw materials of the mortar layer also include 0.05-0.5 parts of defoaming agent.

7. The anticorrosive coating for ductile iron pipe according to claim 6, characterized in that: The defoamer is at least one of a silicon defoamer, a polyether defoamer, a high-carbon alcohol defoamer, a mineral oil defoamer or a vegetable oil defoamer.

8. The anticorrosive coating for ductile iron pipe according to claim 1, characterized in that: The raw materials of the mortar layer also include 0.1 to 3 parts of retarder.

9. The anticorrosive coating for ductile iron pipe according to claim 8, characterized in that: The retarder is one or more of tartaric acid, sodium gluconate or boric acid.

10. The anticorrosive coating for ductile iron pipe according to any one of claims 1 to 9, characterized in that: The epoxy resin coating is a water-based epoxy resin; and / or The glass fiber mesh cloth is a self-adhesive mesh cloth with a mesh size of 2-4 mm.

11. The anticorrosive coating for ductile iron pipe according to any one of claims 1 to 9, characterized in that: The cement is one of silicate cement or aluminate cement; and / or The fiber is one of polypropylene fiber or glass fiber; and / or The thickening and dispersing agent is cellulose.

12. The anticorrosive coating for ductile iron pipe according to claim 11, characterized in that: The strength grade of the silicate cement is one of 42.5, 42.5R, 52.5 or 52.5R; and / or The mesh size of the sand is not less than 4 meshes; and / or The fiber length is 6 to 9 mm; and / or The viscosity of the thickening dispersant is 50,000 mPa.s to 200,000 mPa.s.

13. A ductile iron pipe, characterized in that: The invention comprises the anti-corrosion coating for ductile iron pipes as described in any one of claims 1 to 12.

14. The method for preparing the anticorrosive coating of a ductile iron pipe according to any one of claims 1 to 12, characterized in that: At least the following steps are included: S1: Weighing each component according to the designed ratio, mixing the solid material and the liquid material respectively to prepare a solid mixed material and a liquid mixed material, and then mixing the solid mixed material and the liquid mixed material to obtain a mortar layer raw material mixture; S2: preparing a connection layer on the outer surface of the ductile iron pipe; S3: spraying the mortar layer raw material mixture onto the connection layer surface of the ductile iron pipe respectively, grinding and curing, and obtaining the ductile iron pipe anti-corrosion coating.

15. The preparation method according to claim 14, characterized in that: In S1, if the raw materials of the mortar layer include only basic components, the solid mixed material is a material obtained by mixing cement, sand, thickening dispersant, water reducing agent, thixotropic lubricant and fiber, and the liquid mixed material is water; If the raw materials of the mortar layer also include a retarder or a waterproofing agent, the solid mixed material is a material obtained by mixing the retarder or the waterproofing agent with a basic component other than water, and the liquid phase material is water; If the raw materials of the mortar layer also include emulsion or defoamer, the liquid phase mixed material is a material obtained by mixing the emulsion or defoamer with water.

16. The preparation method according to claim 14, characterized in that: In S3, the quick-setting agent and the mortar layer raw material mixture can also be sprayed onto the surface of the connecting layer of the ductile iron pipe, polished and cured to obtain the ductile iron pipe anti-corrosion coating.

17. The preparation method according to claim 16, characterized in that: The accelerating setting agent is one or more of an alkaline earth metal carbonate accelerating setting agent, a composite sulphoaluminate accelerating setting agent or an aluminate accelerating setting agent.

18. The preparation method according to any one of claims 14 or 16, characterized in that: After curing in S3, the step of coating the infiltration crystallization agent on the surface of the ductile iron pipe is also included.

19. The preparation method according to claim 18, characterized in that: The penetrating crystallization agent is Pengneichuan concrete protective agent PNC701.

Citation Information

Patent Citations

  • Coating raw material composition, nodular cast iron pipe and preparation method therefor

    CN105384417A

  • Cement-based anti-seepage and anti-corrosion multi-layer coating and application method thereof

    CN114058239A

  • Pipeline polymer mortar inside lining of site operation