Hot rolled steel plate
By controlling the chemical composition and structural structure of hot-rolled steel plates and combining with specific hot-rolling process conditions, the problems of high strength and excellent ductility are solved, and tensile strength and shear processing are achieved above 980MPa, which is suitable for high-performance components .
Patent Information
- Application Number
- CN202180056206.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-27
- Filing Date
- 2021-06-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-06-15
AI Technical Summary
The prior art is difficult to take into account high strength, excellent ductility and shear processing properties. Especially in high-strength steel plate applications with a strength of more than 980MPa, steel plates with a strength of less than 850MPa are difficult to meet the needs of automotive components.
By controlling the chemical composition and metal structure of hot-rolled steel plates, it includes martensite, bainite and appropriate amount of ferrite, and implementing intermediate air cooling in the hot-rolling process, controlling the standard deviation of Mn concentration, and reducing the period of structure morphology in the hot-rolling process. and uniformity, combined with specific hot rolling and cooling conditions, steel plates with tensile strength of 980MPa or above were prepared.
It achieves high performance raw materials suitable for automobiles and mechanical components while maintaining excellent ductility and shear processing properties, and suppressing internal cracking in bending.
Smart Images

Figure BDA0004113322710000151 
Figure BDA0004113322710000152 
Figure BDA0004113322710000251
Abstract
Description
Technical Field
[0001] The present invention relates to a hot-rolled steel sheet, and more specifically to a hot-rolled steel sheet that is formed into various shapes by press working or the like and is used, and particularly to a hot-rolled steel sheet that is high in strength and excellent in ductility and shear workability.
[0002] This application claims priority based on Japanese Patent Application No. 2020-143743 filed in Japan on August 27, 2020, the contents of which are incorporated herein by reference. Background Art
[0003] In recent years, efforts have been made to reduce carbon dioxide emissions in many fields from the perspective of protecting the global environment. Automobile manufacturers have also actively developed technologies to reduce vehicle body weight for the purpose of reducing fuel consumption. However, in order to ensure the safety of passengers, the focus is still on improving collision resistance, so it is not easy to reduce the weight of the vehicle body.
[0004] In order to take into account both lightweight vehicle bodies and collision resistance, the use of high-strength steel plates to thin the walls of components has been studied. Therefore, there is a strong desire for steel plates that have both high strength and excellent formability, and several technologies have been proposed in the past to meet these requirements. Since there are various processing styles for automotive components, the required formability varies depending on the components to be applied, among which ductility is positioned as an important indicator of formability. In addition, automotive components are formed by press forming, but the press-formed blank plates are mostly manufactured by shearing with high productivity. For blank plates manufactured by shearing, it is necessary to make the end face accuracy after shearing excellent. For example, if the ratio of the shear surface to the end face after shearing (shear end face) (hereinafter referred to as the shear surface ratio) is unstable (the change in the shear surface ratio is large), the accuracy of the shear end face will deteriorate significantly.
[0005] Regarding the technology for improving ductility, for example, Patent Document 1 discloses a high-strength steel sheet for automobiles with excellent collision safety and formability, wherein retained austenite with an average grain size of 5 μm or less is dispersed in ferrite with an average grain size of 10 μm or less. In the case of a steel sheet containing retained austenite in the metal structure, although austenite undergoes martensitic transformation during processing and shows a large elongation due to phase transformation plasticity, the hole expandability is impaired due to the formation of hard martensite. Patent Document 1 discloses that by refining ferrite and retained austenite, not only ductility but also hole expandability is improved.
[0006] Patent Document 2 discloses a high-strength steel sheet having excellent ductility and stretch flangeability and having a tensile strength of 980 MPa or more, wherein a second phase composed of retained austenite and / or martensite is finely dispersed within a crystal grain.
[0007] Regarding the technology for improving shear workability, for example, Patent Document 3 discloses a technology in which the ferrite grain size d of the surface layer is reduced to s The ferrite crystal grains inside b The ratio d s / d b Control it to below 0.95 to control the fin height after punching.
[0008] Patent Document 4 discloses a technique for improving peeling and warping of the sheet end surface by reducing the P content.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 11-61326
[0012] Patent Document 2: Japanese Patent Application Publication No. 2005-179703
[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 10-168544
[0014] Patent Document 4: Japanese Patent Application Publication No. 2005-298924
[0015] Non-patent literature
[0016] Non-patent document 1: J. Webel, J. Gola, D. Britz, F. Mucklich, Materials Characterization 144 (2018) pp. 584-596
[0017] Non-patent document 2: DL Naik, HUSajid, R. Kiran, Metals 2019, 9, 546
[0018] Non-patent document 3: K. Zuiderveld, Contrast Limited Adaptive Histogram Equalization, Chapter VIII.5, Graphics Gems IV. P. S. Heckbert (Eds.), Cambridge, MA, Academic Press, 1994, pp. 474-485 Summary of the invention
[0019] Problems to be solved by the invention
[0020] The technologies disclosed in Patent Documents 1 to 4 are all technologies for improving either ductility or the end surface properties after shearing. However, in Patent Documents 1 to 3, there is no mention of a technology for taking these properties into consideration. In Patent Document 4, there is a mention of taking shearing workability and press formability into consideration. However, the strength of the steel plate disclosed in Patent Document 4 is lower than 850 MPa, so it may be difficult to apply to high-strength components of 980 MPa or more.
[0021] The present invention has been made in view of the above-mentioned problems in the prior art, and an object of the present invention is to provide a hot-rolled steel sheet having high strength and excellent ductility and shear workability.
[0022] Means for solving problems
[0023] In view of the above-mentioned problems, the inventors of the present invention have repeatedly conducted in-depth studies on the chemical composition and metal structure of hot-rolled steel sheets and the relationship between mechanical properties, and as a result, obtained the following insights (a) to (i), thereby completing the present invention. It should be noted that the so-called excellent shear workability means that the shear surface ratio occupied by the shear end surface is stable, that is, the change in the shear surface ratio is small. In addition, the so-called excellent strength or high strength means that the tensile strength is 980MPa or more.
[0024] (a) In order to obtain excellent tensile (maximum) strength, it is preferable to use a hard structure. That is, it is preferable that the metal structure contains martensite and bainite.
[0025] (b) However, since hard structures are structures with insufficient ductility, excellent ductility cannot be ensured simply by making a metal structure mainly composed of them.
[0026] (c) In order to make the high-strength hot-rolled steel sheet have excellent ductility, it is effective to contain an appropriate amount of ferrite having high ductility.
[0027] (d) Ferrite is generally soft, so in order to obtain the desired strength, it is necessary to use Ti, Nb, V, etc. as precipitation strengthening elements. Therefore, it is effective to perform intermediate air cooling during the hot rolling process to obtain an appropriate amount of precipitation-strengthened ferrite.
[0028] (e) In order to stabilize the shear surface ratio in the shear end surface, it is important to have a metal structure in which Mn segregation is small, the structure morphology is irregular without periodicity, and is non-uniform (low uniformity).
[0029] (f) Specifically, the following are effective for stabilizing the shear surface ratio in the shear end surface: setting the standard deviation of the Mn concentration to a certain value or less; and controlling the periodicity and uniformity of the metal structure.
[0030] (g) In order to set the standard deviation of the Mn concentration to a certain value or less, the slab heating process and the subsequent hot rolling process are important. For example, the following are effective: maintaining the slab in a temperature range of 700 to 850°C for more than 900 seconds, then further heating, maintaining the slab in a temperature range of 1100°C or more for more than 6000 seconds; and performing hot rolling in a temperature range of 850°C to 1100°C to reduce the slab thickness by more than 90% in total.
[0031] (h) In order to reduce the periodicity of the microstructure, it is important to control the recrystallization behavior of austenite during hot rolling. For example, the following items are effective: the reduction ratio and rolling temperature of the final stage of hot rolling are controlled within a specified range, the stress applied to the steel plate after the first stage of the final stage of hot rolling and before the final stage of hot rolling is set to 170 kPa or more, and the stress applied to the steel plate after the final stage of hot rolling and before the steel plate is cooled to 800°C is set to less than 200 kPa. Through such hot rolling conditions, fine and equiaxed recrystallized austenite grains can be produced, and by combining with the subsequent cooling conditions, the periodicity of the microstructure can be reduced.
[0032] (i) In order to reduce the uniformity of the metal structure, it is effective to perform intermediate air cooling to obtain a desired amount of ferrite and then cool to a temperature range of 400° C. or higher and lower than 650° C. to suppress precipitation of iron carbides.
[0033] The gist of the present invention made based on the above findings is as follows.
[0034] (1) The chemical composition of the hot-rolled steel sheet according to one embodiment of the present invention contains, in terms of mass %, the following:
[0035] C: 0.050~0.250%,
[0036] Si: 0.05-3.00%,
[0037] Mn: 1.00~4.00%,
[0038] One or more of Ti, Nb and V: 0.060 to 0.500% in total,
[0039] Sol.Al: 0.001~2.000%,
[0040] P: 0.100% or less,
[0041] S: 0.0300% or less,
[0042] N: 0.1000% or less,
[0043] O: 0.0100% or less,
[0044] Cu: 0-2.00%,
[0045] Cr: 0~2.00%,
[0046] Mo: 0-1.00%,
[0047] Ni: 0-2.00%,
[0048] B: 0~0.0100%,
[0049] Ca: 0~0.0200%,
[0050] Mg: 0~0.0200%,
[0051] REM: 0~0.1000%、
[0052] Bi: 0~0.020%,
[0053] One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and
[0054] Sn: 0~0.05%,
[0055] The rest contains Fe and impurities.
[0056] The metal structure is as follows:
[0057] In terms of area%, the retained austenite is less than 3.0%, the ferrite is 15.0% or more and less than 60.0%, and the pearlite is less than 5.0%;
[0058] The E value indicating the periodicity of the metal structure is greater than 10.7, and the I value indicating the uniformity of the metal structure is less than 1.020;
[0059] The standard deviation of the Mn concentration is 0.60 mass % or less,
[0060] The tensile strength is above 980 MPa.
[0061] (2) The hot-rolled steel sheet according to (1) above, wherein the average grain size of the surface layer may be less than 3.0 μm.
[0062] (3) The hot-rolled steel sheet according to (1) or (2), wherein the chemical composition may contain, in terms of mass %, one or more elements selected from the following:
[0063] Cu: 0.01-2.00%,
[0064] Cr: 0.01~2.00%,
[0065] Mo: 0.01~1.00%,
[0066] Ni: 0.02-2.00%,
[0067] B: 0.0001~0.0100%,
[0068] Ca: 0.0005~0.0200%,
[0069] Mg: 0.0005~0.0200%,
[0070] REM: 0.0005~0.1000%, and
[0071] Bi: 0.0005~0.020%.
[0072] Effects of the Invention
[0073] According to the above embodiment of the present invention, a hot rolled steel sheet having excellent strength, ductility and shear workability can be obtained. In addition, according to the above preferred embodiment of the present invention, a hot rolled steel sheet having the above characteristics and suppressing the occurrence of bending cracking, i.e., excellent bending cracking resistance can be obtained.
[0074] The hot-rolled steel sheet of the present invention is suitable as an industrial raw material used in automobile components, mechanical structural components, and even building components. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 This is a diagram for explaining a method for measuring the ratio of the sheared surface to the end surface after shearing. DETAILED DESCRIPTION
[0076] The chemical composition and metal structure of the hot rolled steel sheet (hereinafter sometimes referred to as steel sheet) of this embodiment are described in more detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various changes can be made within the scope of the present invention.
[0077] Regarding the numerical ranges described below with "to", the lower limit and the upper limit are included in the range. Regarding the numerical values expressed as "lower than" or "exceeding", the value is not included in the numerical range. In the following description, "%" about the chemical composition of the steel plate means "mass %" unless otherwise specified.
[0078] 1. Chemical composition
[0079] The hot rolled steel sheet of the present embodiment contains, by mass%, C: 0.050-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, one or more of Ti, Nb and V: 0.060-0.500% in total, sol.Al: 0.001-2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, and the remainder: Fe and impurities. Each element is described in detail below.
[0080] (1-1) C: 0.050~0.250%
[0081] C increases the hard phase fraction and combines with precipitation strengthening elements such as Ti, Nb, and V to increase the strength of ferrite. When the C content is less than 0.050%, it becomes difficult to obtain the desired strength. Therefore, the C content is set to 0.050% or more. The C content is preferably 0.060% or more, more preferably 0.070% or more, and even more preferably 0.080% or more.
[0082] On the other hand, when the C content exceeds 0.250%, the ductility of the hot-rolled steel sheet decreases due to the decrease in the fraction of ferrite. Therefore, the C content is set to 0.250% or less. The C content is preferably 0.150% or less.
[0083] (1-2) Si: 0.05-3.00%
[0084] Si has the following effects: promoting the formation of ferrite to improve the ductility of hot-rolled steel sheets; and strengthening ferrite by solid solution to increase the strength of hot-rolled steel sheets. In addition, Si has the effect of making steel sound by deoxidation (suppressing the generation of defects such as pores in steel). When the Si content is less than 0.05%, the effects brought about by the above effects cannot be obtained. Therefore, the Si content is set to 0.05% or more. The Si content is preferably 0.50% or more, and more preferably 0.80% or more.
[0085] However, when the Si content exceeds 3.00%, the surface properties and chemical conversion treatability of the steel sheet, and further the ductility and weldability, are significantly deteriorated, and A 3 The transformation point rises significantly. As a result, it becomes difficult to perform hot rolling stably. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.70% or less, and more preferably 2.50% or less.
[0086] (1-3) Mn: 1.00~4.00%
[0087] Mn has the effect of suppressing ferrite transformation and increasing the strength of the hot-rolled steel sheet. When the Mn content is less than 1.00%, a tensile strength of 980 MPa or more cannot be obtained. Therefore, the Mn content is set to 1.00% or more. The Mn content is preferably 1.30% or more, and more preferably 1.50% or more.
[0088] On the other hand, when the Mn content exceeds 4.00%, the hard phase becomes a periodic band due to the segregation of Mn, and it becomes difficult to obtain the desired shear workability. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, and more preferably 3.50% or less.
[0089] (1-4) One or more of Ti, Nb and V: 0.060 to 0.500% in total
[0090] Ti, Nb and V are elements that precipitate finely in steel as carbides and nitrides and improve the strength of steel by precipitation strengthening. In addition, they are elements that fix C by forming the above-mentioned carbides and suppress the formation of cementite that is harmful to shear workability. If the total content of Ti, Nb and V is less than 0.060%, these effects cannot be obtained. Therefore, the total content of Ti, Nb and V is set to more than 0.060%. It should be noted that it is not necessary to contain Ti, Nb and V, as long as any one of them is contained, and the total content is more than 0.060%. The total content of Ti, Nb and V is preferably more than 0.080%, and more preferably more than 0.100%.
[0091] On the other hand, if the total content of Ti, Nb and V exceeds 0.500%, workability deteriorates. Therefore, the total content of Ti, Nb and V is set to 0.500% or less, preferably 0.300% or less, more preferably 0.250% or less, and further preferably 0.200% or less.
[0092] (1-5)sol.Al: 0.001~2.000%
[0093] Al, like Si, has the function of deoxidizing steel to make it sound, and has the function of promoting the formation of ferrite to improve the ductility of hot-rolled steel sheets. When the sol.Al content is less than 0.001%, the effects brought about by the above-mentioned functions cannot be obtained. Therefore, the sol.Al content is set to 0.001% or more. The sol.Al content is preferably 0.010% or more.
[0094] On the other hand, when the sol.Al content exceeds 2.000%, the above effect is saturated and it is not economically preferable, so the sol.Al content is set to 2.000% or less. The sol.Al content is preferably 1.500% or less, more preferably 1.300% or less, and further preferably 1.000% or less.
[0095] It should be noted that sol.Al refers to acid-soluble Al, and means solid-solution Al present in the steel in a solid-solution state.
[0096] (1-6) P: 0.100% or less
[0097] P is an element generally contained as an impurity, but it is also an element that has the effect of improving the strength of the hot-rolled steel sheet by solid solution strengthening. Therefore, P can also be actively contained, but P is an element that is easy to segregate. If the P content exceeds 0.100%, the reduction in ductility caused by grain boundary segregation becomes significant. Therefore, the P content is limited to 0.100% or less. The P content is preferably 0.030% or less. The lower limit of the P content does not need to be specifically specified, but from the perspective of refining cost, it is preferably set to 0.001%.
[0098] (1-7) S: 0.0300% or less
[0099] S is an element contained as an impurity, and forms sulfide-based inclusions in steel to reduce the ductility of the hot-rolled steel sheet. If the S content exceeds 0.0300%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the S content is limited to 0.0300% or less. The S content is preferably 0.0050% or less. The lower limit of the S content does not need to be specifically specified, but from the viewpoint of refining cost, it is preferably set to 0.0001%.
[0100] (1-8) N: 0.1000% or less
[0101] N is an element contained in steel as an impurity, and has the effect of reducing the ductility of the hot-rolled steel sheet. When the N content exceeds 0.1000%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, more preferably 0.0700% or less, and further preferably 0.0100% or less. There is no need to specifically specify the lower limit of the N content, but in the case of containing one or more of Ti, Nb and V to make the metal structure more refined, in order to promote the precipitation of carbonitrides, the N content is preferably set to 0.0010% or more, and more preferably 0.0020% or more.
[0102] (1-9) O: 0.0100% or less
[0103] If a large amount of O is contained in the steel, coarse oxides that become the starting point of fracture will be formed, causing brittle fracture and hydrogen cracking. Therefore, the O content is set to 0.0100% or less. The O content is preferably 0.0080% or less, and more preferably 0.0050% or less. In order to disperse a large amount of fine oxides during deoxidation of the molten steel, the O content may be set to 0.0005% or more, or 0.0010% or more.
[0104] The remainder of the chemical composition of the hot-rolled steel sheet of the present embodiment may also be Fe and impurities. In the present embodiment, the so-called impurities refer to substances mixed from ore, waste materials or manufacturing environment as raw materials, and / or substances allowed within the range that do not adversely affect the hot-rolled steel sheet of the present embodiment.
[0105] The hot-rolled steel sheet of the present embodiment may contain Cu, Cr, Mo, Ni, B, Ca, Mg, REM, Bi, Zr, Co, Zn, W and Sn as optional elements to replace a part of Fe. The lower limit of the content when the optional elements are not contained is 0%. The optional elements are described in detail below.
[0106] (1-10)Cu: 0.01~2.00%, Cr: 0.01~2.00%, Mo: 0.01~1.00%, Ni: 0.02~2.00% and B: 0.0001~0.0100%
[0107] Cu, Cr, Mo, Ni and B all have the effect of improving the hardenability of the hot-rolled steel sheet. In addition, Cu and Mo have the effect of precipitating as carbides in the steel to improve the strength of the hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing the grain boundary cracking of the slab caused by Cu. Therefore, one or more of these elements may also be contained.
[0108] Cu has the following effects: improving the hardenability of hot-rolled steel sheets; and precipitating as carbides in steel at low temperatures to improve the strength of hot-rolled steel sheets. In order to more reliably obtain the effects brought about by the above effects, the Cu content is preferably set to 0.01% or more, and more preferably set to 0.05% or more. However, when the Cu content exceeds 2.00%, grain boundary cracking of the slab may occur. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, and more preferably 1.00% or less.
[0109] As mentioned above, Cr has the effect of improving the hardenability of hot-rolled steel sheets. In order to more reliably obtain the effect brought about by the above-mentioned effect, it is preferred to set the Cr content to 0.01% or more, and more preferably to 0.05% or more. However, when the Cr content exceeds 2.00%, the chemical conversion treatability of the hot-rolled steel sheet is significantly reduced. Therefore, the Cr content is set to 2.00% or less.
[0110] As described above, Mo has the following effects: improving the hardenability of hot-rolled steel sheets; and improving the strength of hot-rolled steel sheets by precipitating as carbides in steel. In order to more reliably obtain the effects brought about by the above effects, it is preferred that the Mo content be set to 0.01% or more, and more preferably to 0.02% or more. However, even if the Mo content is set to more than 1.00%, the effects brought about by the above effects are saturated, which is not economically preferred. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, and more preferably 0.20% or less.
[0111] As described above, Ni has the effect of improving the hardenability of hot-rolled steel sheets. In addition, when Cu is contained, Ni has the effect of effectively suppressing the grain boundary cracking of the slab caused by Cu. In order to more reliably obtain the effect brought about by the above-mentioned effect, the Ni content is preferably set to 0.02% or more. Ni is an expensive element, so it is not economically preferable to contain a large amount of Ni. Therefore, the Ni content is set to 2.00% or less.
[0112] As mentioned above, B has the effect of improving the hardenability of the hot-rolled steel sheet. In order to more reliably obtain the effect brought about by this effect, it is preferred to set the B content to 0.0001% or more, and more preferably to 0.0002% or more. However, when the B content exceeds 0.0100%, the formability of the hot-rolled steel sheet is significantly reduced, so the B content is set to 0.0100% or less. The B content is preferably set to 0.0050% or less.
[0113] (1-11) Ca: 0.0005 to 0.0200%, Mg: 0.0005 to 0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005 to 0.020%
[0114] Ca, Mg and REM all have the effect of improving the ductility of the hot-rolled steel sheet by adjusting the shape of the inclusions in the steel to a preferred shape. In addition, Bi has the effect of improving the ductility of the hot-rolled steel sheet by refining the solidification structure. Therefore, one or more of these elements may also be contained. In order to more reliably obtain the effects brought about by the above-mentioned effects, it is preferred to set any one or more of Ca, Mg, REM and Bi to 0.0005% or more. However, if the Ca content or the Mg content exceeds 0.0200%, or the REM content exceeds 0.1000%, it is possible that inclusions are excessively generated in the steel, which in turn reduces the ductility of the hot-rolled steel sheet. In addition, even if the Bi content is set to more than 0.020%, the effect brought about by the above-mentioned effects is saturated, which is not economically preferred. Therefore, the Ca content and the Mg content are set to less than 0.0200%, the REM content is set to less than 0.1000%, and the Bi content is set to less than 0.020%. The Bi content is preferably 0.010% or less.
[0115] Here, REM refers to a total of 17 elements including Sc, Y and lanthanoid elements, and the above-mentioned REM content refers to the total content of these elements. In the case of lanthanoid elements, they are added in the form of mixed rare earth alloys in industry.
[0116] (1-12) One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0 to 0.05%
[0117] Regarding Zr, Co, Zn and W, the inventors of the present invention have confirmed that even if these elements are contained in an amount of 1.00% or less in total, the effect of the hot-rolled steel sheet of the present embodiment is not impaired. Therefore, one or more of Zr, Co, Zn and W may be contained in an amount of 1.00% or less in total.
[0118] The inventors of the present invention have confirmed that even if a small amount of Sn is contained, the effect of the hot-rolled steel sheet of the present embodiment is not impaired. However, if a large amount of Sn is contained, there is a possibility that defects will occur during hot rolling, so the Sn content is set to 0.05% or less.
[0119] The chemical composition of the hot-rolled steel sheet mentioned above can be measured by general analytical methods. For example, it can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). In addition, sol.Al can be measured by ICP-AES using the filtrate after the sample is heated and decomposed with acid. C and S can be measured by the combustion-infrared absorption method, N can be measured by the inert gas melting-thermal conductivity method, and O can be measured by the inert gas melting-non-dispersive infrared absorption method.
[0120] 2. Metal structure of hot rolled steel plate
[0121] Next, the metal structure of the hot-rolled steel sheet according to the present embodiment will be described.
[0122] The metal structure of the hot-rolled steel sheet of the present embodiment is less than 3.0% of retained austenite in terms of area%, ferrite is more than 15.0% and less than 60.0%, pearlite is less than 5.0%, the E value representing the periodicity of the above-mentioned metal structure is more than 10.7, the I value representing the uniformity of the above-mentioned metal structure is less than 1.020, and the standard deviation of the Mn concentration is less than 0.60 mass%. Therefore, the hot-rolled steel sheet of the present embodiment can obtain high strength, excellent ductility and shear workability. It should be noted that in the present embodiment, in a cross section parallel to the rolling direction, the standard deviation of the structure fraction, E value, I value and Mn concentration in the metal structure at a depth of 1 / 4 of the plate thickness from the surface and at the center of the plate width direction is specified. The reason is that the metal structure at this position represents the representative metal structure of the steel plate.
[0123] (2-1) Area fraction of retained austenite: less than 3.0%
[0124] Retained austenite is a metal structure that exists in the form of a face-centered cubic lattice even at room temperature. Retained austenite has the effect of improving the ductility of the hot-rolled steel sheet through phase transformation plasticity (TRIP). On the other hand, since the retained austenite transforms into high-carbon martensite during shearing, it will hinder the generation of stable cracks and become the cause of the instability of the shear surface ratio occupied in the shear end face. When the area fraction of retained austenite is more than 3.0%, the above-mentioned effect becomes obvious, and the shear workability of the hot-rolled steel sheet deteriorates. Therefore, the area fraction of retained austenite is set to less than 3.0%. The area fraction of retained austenite is preferably less than 1.5%, and more preferably less than 1.0%. The less retained austenite, the better, so the area fraction of retained austenite can also be 0%.
[0125] The area fraction of retained austenite can be measured by X-ray diffraction, EBSP (Electron Back Scattering Diffraction Pattern) analysis, magnetic measurement, etc. The measured values may differ depending on the measurement method. In the present embodiment, the area fraction of retained austenite is measured by X-ray diffraction.
[0126] In the measurement of the area fraction of retained austenite by X-ray diffraction in the present embodiment, first, in a cross section parallel to the rolling direction at a depth of 1 / 4 of the plate thickness of the hot-rolled steel plate (a region from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface) and at the center of the plate width direction, Co-Kα rays are used to determine the integrated intensity of a total of six peaks, α(110), α(200), α(211), γ(111), γ(200), and γ(220), and the intensity average method is used to calculate the area fraction of retained austenite.
[0127] (2-2) Area fraction of ferrite: 15.0% or more and less than 60.0%
[0128] Ferrite is a structure formed when fcc transforms to bcc at a relatively high temperature. Ferrite has a high work hardening rate, so it has the effect of improving the strength-ductility balance of hot-rolled steel sheets. In order to obtain the above effect, the area fraction of ferrite is set to 15.0% or more. It is preferably 20.0% or more, more preferably 25.0% or more, and even more preferably 30.0% or more.
[0129] On the other hand, since ferrite has low strength, if the area fraction is excessive, the desired tensile strength cannot be obtained. Therefore, the area fraction of ferrite is set to be less than 60.0%, preferably 50.0% or less, and more preferably 45.0% or less.
[0130] (2-3) Area fraction of pearlite: less than 5.0%
[0131] Pearlite is a lamellar metal structure in which cementite is precipitated in layers between ferrites, and is a softer metal structure than bainite and martensite. If the area fraction of pearlite is 5.0% or more, carbon is consumed by cementite contained in pearlite, and the strength of martensite and bainite as the remaining structures decreases, and a tensile strength of 980 MPa or more cannot be obtained. Therefore, the area fraction of pearlite is set to less than 5.0%. The area fraction of pearlite is preferably 3.0% or less. In order to improve the stretch flangeability of the steel plate, the area fraction of pearlite is preferably reduced as much as possible, and the area fraction of pearlite is more preferably 0%.
[0132] In addition, in the steel sheet of this embodiment, as the remaining structure other than retained austenite, ferrite and pearlite, one or more hard structures of bainite, martensite and tempered martensite are included with a total area fraction of more than 32.0% and 85.0% or less.
[0133] The area fraction of the metal structure is measured by the following method. The cross section parallel to the rolling direction is finished into a mirror surface, and the strain introduced into the surface layer of the sample is removed by grinding for 8 minutes at room temperature using colloidal silica without alkaline solution. At any position in the length direction of the sample cross section, an area with a length of 50 μm, a depth of 1 / 4 of the plate thickness from the surface (an area with a depth of 1 / 8 of the plate thickness from the surface to a depth of 3 / 8 of the plate thickness from the surface), and a central position in the plate width direction is measured by electron backscatter diffraction at a measurement interval of 0.1 μm to obtain crystal orientation information. For the measurement, an EBSD analysis device consisting of a thermal field emission scanning electron microscope (JSM-7001F manufactured by JEOL) and an EBSD detector (DVC5 detector manufactured by TSL) is used. At this time, the vacuum degree in the EBSD analysis device is set to 9.6×10 -5 Pa or less, the acceleration voltage was set to 15 kV, the irradiation current level was set to 13, and the electron beam irradiation level was set to 62.
[0134] Furthermore, a reflected electron image is taken in the same field of view. First, the crystal grains in which ferrite and cementite are precipitated in layers are determined by the reflected electron image, and the area fraction of pearlite is obtained by calculating the area fraction of the crystal grains. Afterwards, for the crystal grains other than the crystal grains determined as pearlite, the obtained crystal orientation information is used using the "Grain Average Misorientation (grain average orientation difference)" function carried in the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device, and the area with a Grain Average Misorientation value of less than 1.0° is determined as ferrite. The area fraction of ferrite is obtained by obtaining the area fraction of the area determined as ferrite.
[0135] Next, under the condition that the 5° grain boundary in the remaining area (the area where the Grain Average Misorientation value exceeds 1.0°) is defined as the crystal grain boundary, when the maximum value of the "Grain Average IQ" of the ferrite area is set to Iα, the area exceeding Iα / 2 is extracted as bainite, and the area below Iα / 2 is extracted as "pearlite, martensite and tempered martensite". The area fraction of bainite is obtained by calculating the area fraction of the extracted bainite. In addition, the area fraction of the extracted "pearlite, martensite and tempered martensite" is calculated and the area fraction of pearlite obtained by the above-mentioned EBSD analysis is subtracted, thereby obtaining the total area fraction of martensite and tempered martensite.
[0136] (2-4) E value: 10.7 or above, I value: less than 1.020
[0137] In order to stabilize the shear surface ratio in the shear end face, it is important to reduce the periodicity of the metal structure and the uniformity of the metal structure. In this embodiment, the shear surface ratio in the shear end face is stabilized by controlling the E (entropy) value representing the periodicity of the metal structure and the I (inverse differenced moment norm) value representing the uniformity of the metal structure.
[0138] The E value represents the periodicity of the metal structure. When the brightness is arranged periodically due to the formation of a banded structure, that is, when the periodicity of the metal structure is high, the E value decreases. In the present embodiment, since it is necessary to make a metal structure with low periodicity, it is necessary to increase the E value. If the E value is lower than 10.7, the shear surface ratio occupied in the shear end face becomes easily unstable. With the periodically arranged structure as the starting point, cracks are generated from the blade tip of the shear tool in the very early stage of the shearing process to form a fracture surface, and then the shear surface is formed. From this, it is inferred that: the shear surface ratio occupied in the shear end face becomes easily unstable. Therefore, the E value is set to be greater than 10.7. Preferably, it is greater than 10.8, and more preferably, it is greater than 11.0. The higher the E value, the more preferred it is. There is no particular upper limit, but it can also be set to less than 13.0, less than 12.5, or less than 12.0.
[0139] The I value represents the uniformity of the metal structure, and the wider the area of the region with a certain brightness, the higher it rises. A high I value means that the uniformity of the metal structure is high. In the present embodiment, since it is necessary to make a metal structure with low uniformity of the metal structure, it is necessary to reduce the I value. If the I value is low and the uniformity of the metal structure is low, it becomes easy to produce cracks from the front end of the shearing tool due to the influence of the precipitates in the crystal and the hardness difference caused by the difference in element concentration, and the shear surface ratio can be stabilized. It is estimated that if the I value is above 1.020, the shear surface ratio occupied in the shear end face cannot be stabilized. Therefore, the I value is set to be lower than 1.020. Preferably, it is below 1.015, and more preferably below 1.010. The lower limit of the I value is not particularly specified, but it can also be set to above 0.900, above 0.950 or above 1.000.
[0140] The E value and the I value can be obtained by the following method.
[0141] In this embodiment, the shooting area of the SEM image taken to calculate the E value and the I value is set to: a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in a cross section parallel to the rolling direction (an area from 1 / 8 of the plate thickness to 3 / 8 of the plate thickness from the surface), and a central position in the plate width direction. For the shooting of the SEM image, a SU-6600 Schottky electron gun manufactured by Hitachi High-Technologies Corporation was used, the emitter was set to tungsten, and the acceleration voltage was set to 1.5 kV. Based on the above settings, the SEM image was output at a magnification of 1000 times and a gray scale of 256 gray levels.
[0142] Next, the obtained SEM image was cut into an area of 880×880 pixels and the image was subjected to a smoothing process with a block grid size of 8×8 and a contrast enhancement limit ratio of 2.0 as described in non-patent document 3. The smoothed SEM image was rotated counterclockwise at every 1 degree from 0 to 179 degrees except for 90 degrees, and a total of 179 images were obtained by making images at every 1 degree. Next, for each of these 179 images, the frequency values of the brightness between adjacent pixels were collected in the form of rows and columns using the GLCM method described in non-patent document 1.
[0143] For the 179 frequency value rows and columns collected by the above method, k is set to the rotation angle with the original image, expressed as p k (k=0...89, 91, ...179). For each image, the generated p kAfter summing up all k (k=0...89, 91...179), a 256×256 matrix P normalized so that the sum of each component becomes 1 is calculated. Furthermore, the E value and I value are calculated using the following equations (1) and (2) described in Non-Patent Document 2, respectively.
[0144] In the following equations (1) and (2), the value of the i-th row and j-th column of the row P is expressed as P ij .
[0145]
[0146]
[0147] (2-5) Standard deviation of Mn concentration: 0.60 mass % or less
[0148] The standard deviation of the Mn concentration at the central position of the hot-rolled steel sheet of this embodiment, which is 1 / 4 of the plate thickness from the surface and in the plate width direction, is 0.60% by mass or less. As a result, the hard phase can be evenly dispersed, and cracks can be prevented from occurring from the tip of the shearing tool at an extremely early stage of the shearing process. As a result, the shear surface ratio occupied in the shear end face can be stabilized. The standard deviation of the Mn concentration is preferably 0.50% by mass or less, and more preferably 0.47% by mass or less. From the viewpoint of suppressing excessive fins, the lower limit of the standard deviation of the Mn concentration is preferably as small as possible, but due to the constraints of the manufacturing process, the substantive lower limit is 0.10% by mass.
[0149] After mirror polishing the cross section (L cross section) of the hot-rolled steel plate parallel to the rolling direction, the steel plate is measured with an electron probe microanalyzer (EPMA) at a depth of 1 / 4 of the plate thickness from the surface (the area from 1 / 8 of the plate thickness to 3 / 8 of the plate thickness from the surface) and the center position in the plate width direction to determine the standard deviation of the Mn concentration. The measurement conditions are to set the acceleration voltage to 15 kV, set the magnification to 5000 times, and measure the distribution image of the range of 20 μm in the rolling direction of the sample and 20 μm in the plate thickness direction of the sample. More specifically, the measurement interval is set to 0.1 μm, and the Mn concentration is measured at more than 40,000 locations. Next, the standard deviation of the Mn concentration is obtained by calculating the standard deviation based on the Mn concentration obtained from all the measurement points.
[0150] (2-6) Average crystal grain size of the surface layer: less than 3.0 μm
[0151] By making the crystal grain size of the surface layer fine, the in-bend cracking of the hot-rolled steel sheet can be suppressed. The higher the strength of the steel sheet becomes, the easier it is to generate cracks from the inside of the bend during the bending process (hereinafter referred to as in-bend cracking). The mechanism of in-bend cracking is estimated as follows. During the bending process, compressive stress is generated on the inside of the bend. Initially, the processing progresses while the entire inside of the bend is deformed uniformly, but if the processing amount becomes larger, the deformation cannot be borne by uniform deformation alone, and the deformation progresses due to local concentration of strain (generation of shear deformation band). The shear deformation band further grows, thereby generating cracks along the shear band from the inside surface of the bend and growing. It is estimated that the reason why in-bend cracking becomes easier to generate with high strength is that due to the reduction of work hardening ability brought about by high strength, uniform deformation becomes difficult to perform, and deformation becomes more likely to be uneven, thereby generating a shear deformation band in the early stage of processing (or under loose processing conditions).
[0152] Through the research of the inventors of the present invention, it is known that bending cracking becomes significant in steel plates with a tensile strength of 980MPa or above. In addition, the inventors of the present invention found that the finer the crystal grain size of the surface layer of the hot-rolled steel plate, the more the local strain concentration is suppressed, and it becomes more difficult to produce bending cracking. In order to obtain the above-mentioned effect, the average crystal grain size of the surface layer of the hot-rolled steel plate is preferably set to less than 3.0μm. Therefore, in this embodiment, the average crystal grain size of the surface layer can also be set to less than 3.0μm. The average crystal grain size of the surface layer is more preferably less than 2.5μm. The lower limit of the average crystal grain size in the surface area is not specifically specified, but can also be set to 0.5μm.
[0153] It should be noted that the surface layer in the present embodiment refers to a region from the surface of the hot-rolled steel sheet to a position at a depth of 50 μm from the surface.
[0154] The crystal grain size of the surface layer is measured using the EBSP-OIM (Electron Back Scatter Diffraction Pattern-Orientation Image Microscopy) method. The EBSP-OIM method is performed using a device obtained by combining a scanning electron microscope with an EBSP analysis device and OIM Analysis (registered trademark) manufactured by AMETEK. The analyzable area of the EBSP-OIM method is an area that can be observed by SEM. Although it also varies depending on the resolution of the SEM, according to the EBSP-OIM method, the minimum resolution that can be analyzed is 20nm.
[0155] In the cross section of the hot-rolled steel sheet parallel to the rolling direction, the area from the surface of the hot-rolled steel sheet to the area at a depth of 50 μm from the surface and the center of the plate width direction is analyzed at a magnification of 1200 times in an area of 40 μm×30 μm in at least 5 fields of view, and the area where the angle difference between adjacent measurement points is 5° or more is defined as the crystal grain boundary, and the area average crystal grain size is calculated. The obtained area average crystal grain size is taken as the average crystal grain size of the surface layer.
[0156] 3. Tensile strength characteristics
[0157] The tensile strength characteristics (tensile strength, total elongation) of the mechanical properties of the hot-rolled steel sheet were evaluated in accordance with JIS Z 2241: 2011. The test piece was set to the No. 5 test piece of JIS Z 2241: 2011. The sampling position of the tensile test piece was set to be 1 / 4 of the end in the plate width direction, and the direction perpendicular to the rolling direction was set as the length direction.
[0158] The tensile (maximum) strength of the hot-rolled steel sheet of this embodiment is 980 MPa or more. Preferably, it is 1000 MPa or more. If the tensile strength is lower than 980 MPa, the application parts are limited and the contribution to the lightweighting of the vehicle body is small. The upper limit does not need to be particularly limited, but from the perspective of suppressing die wear, it can also be set to 1780 MPa.
[0159] In addition, the total elongation is preferably set to 12.0% or more, and the product of the tensile strength and the total elongation (TS×El) is preferably set to 15000 MPa·% or more. The total elongation is more preferably set to 13.0% or more, and further preferably set to 14.0% or more. In addition, the product of the tensile strength and the total elongation is more preferably set to 15500 MPa·% or more, and further preferably set to 16000 MPa·% or more. By setting the total elongation to 12.0% or more and setting the product of the tensile strength and the total elongation to 15000 MPa·% or more, the application parts are not limited, which can greatly contribute to the lightweighting of the vehicle body.
[0160] 4.Plate thickness
[0161] The plate thickness of the hot-rolled steel plate of the present embodiment is not particularly limited, but can also be set to 1.2 to 8.0 mm. When the plate thickness of the hot-rolled steel plate is less than 1.2 mm, it may be difficult to ensure the rolling completion temperature, and the rolling load becomes too large, making hot rolling difficult. Therefore, the plate thickness of the hot-rolled steel plate of the present embodiment can also be set to 1.2 mm or more. Preferably, it is 1.4 mm or more. On the other hand, when the plate thickness exceeds 8.0 mm, it may be difficult to refine the metal structure and it becomes difficult to obtain the above-mentioned metal structure. Therefore, the plate thickness can also be set to 8.0 mm or less. Preferably, it is 6.0 mm or less.
[0162] 5. Others
[0163] (5-1) Plating
[0164] The hot rolled steel sheet of the present embodiment with the above-mentioned chemical composition and metal structure can also be made into surface treated steel sheet by making the surface have coating for the purpose of improving corrosion resistance. The coating can be an electroplated layer or a hot dip coating. As the electroplated layer, electrogalvanized layer, electroplated Zn-Ni alloy layer, etc. can be exemplified. As the hot dip coating, hot dip galvanized layer, alloyed hot dip galvanized layer, hot dip aluminum layer, hot dip Zn-Al alloy layer, hot dip Zn-Al-Mg alloy layer, hot dip Zn-Al-Mg-Si alloy layer, etc. can be exemplified. The coating adhesion amount is not particularly limited and can be set to be the same as before. In addition, by implementing appropriate chemical conversion treatment (such as coating and drying of chromium-free chemical conversion treatment liquid of silicate system) after plating, corrosion resistance can also be further improved.
[0165] 6. Manufacturing conditions
[0166] A preferred method for producing the hot-rolled steel sheet of the present embodiment having the above-mentioned chemical composition and metal structure is as follows.
[0167] In order to obtain the hot-rolled steel sheet of the present embodiment, it is effective to heat the slab under predetermined conditions, then perform hot rolling, accelerate cooling to a predetermined temperature range, then perform slow cooling, and control the cooling history until coiling.
[0168] In the preferred method for manufacturing the hot-rolled steel sheet of the present embodiment, the following steps (1) to (9) are performed in sequence. It should be noted that the temperature of the slab and the temperature of the steel sheet in the present embodiment refer to the surface temperature of the slab and the surface temperature of the steel sheet. In addition, stress refers to the stress applied along the rolling direction of the steel sheet.
[0169] (1) After the slab is held in a temperature range of 700 to 850° C. for 900 seconds or more, it is further heated and held in a temperature range of 1100° C. or more for 6000 seconds or more.
[0170] (2) Hot rolling is performed in a temperature range of 850 to 1100° C. so that the total thickness reduction is 90% or more.
[0171] (3) A stress of 170 kPa or more is applied to the steel sheet after the rolling one stage before the final stage of hot rolling and before the final stage of rolling.
[0172] (4) The rolling reduction in the final stage of hot rolling is set to 8% or more, and the hot rolling is completed so that the rolling completion temperature Tf becomes 900°C or more and lower than 1010°C.
[0173] (5) The stress applied to the steel sheet after the final stage of hot rolling and before the steel sheet is cooled to 800° C. is set to less than 200 kPa.
[0174] (6) After cooling to a temperature range of 600 to 730°C at an average cooling rate of 50°C / second or more after hot rolling is completed within 1 second, the temperature is accelerated to a temperature range of 50°C to 730°C. Among them, "cooling to a temperature range of 600 to 730°C at an average cooling rate of 50°C / second or more after hot rolling is completed within 1 second" is a more preferred cooling condition.
[0175] (7) Slow cooling is performed in a temperature range of 600 to 730°C for 2.0 seconds or more with an average cooling rate of less than 5°C / second.
[0176] (8) Cooling to a temperature range below 600°C at an average cooling rate of 50°C / s or more.
[0177] (9) Coiling is performed in a temperature range of 400°C or higher and lower than 600°C.
[0178] By adopting the above-mentioned manufacturing method, a hot-rolled steel sheet having a metal structure excellent in strength, ductility and shear workability can be stably manufactured. That is, by appropriately controlling the slab heating conditions and hot rolling conditions, it is possible to reduce the Mn segregation and equiaxed austenite before transformation, and the hot-rolled steel sheet having a desired metal structure can be stably manufactured in conjunction with the cooling conditions after hot rolling described later.
[0179] (6-1) Slab, Slab Temperature and Holding Time during Hot Rolling
[0180] The slabs for hot rolling can be slabs obtained by continuous casting, slabs obtained by casting and slab opening, etc., and slabs obtained by hot working or cold working them as needed can be used. It is preferred that the slabs for hot rolling are kept in a temperature range of 700 to 850°C for more than 900 seconds when the slab is heated, and then further heated and kept in a temperature range of 1100°C or more for more than 6000 seconds. In addition, when the temperature is kept in the temperature range of 700 to 850°C, the temperature of the steel plate can be changed in the temperature range or set to be constant. In addition, when the temperature is kept above 1100°C, the temperature of the steel plate can be changed in the temperature range of 1100°C or more, or set to be constant. In the austenite transformation in the temperature range of 700 to 850°C, Mn is distributed between ferrite and austenite, and by extending its transformation time, Mn can diffuse in the ferrite region. As a result, the Mn microsegregation that is unevenly present in the slab can be eliminated, and the standard deviation of the Mn concentration can be significantly reduced. Furthermore, by maintaining the slab in a temperature range of 1100° C. or higher for 6000 seconds or longer, the austenite grains during the slab heating can be made uniform.
[0181] Hot rolling is preferably performed using a reversing mill or a tandem mill as a multi-pass rolling. In particular, from the viewpoint of industrial productivity and the viewpoint of stress load on the steel plate during rolling, it is more preferable to set at least the last two stages to hot rolling using a tandem mill.
[0182] (6-2) Hot rolling reduction rate: a total thickness reduction of 90% or more in the temperature range of 850 to 1100°C
[0183] By performing hot rolling in a temperature range of 850 to 1100°C to reduce the plate thickness by more than 90%, the recrystallized austenite grains can be mainly refined, and the accumulation of strain energy in the non-recrystallized austenite grains can be promoted. In addition, the recrystallization of austenite can be promoted, and the atomic diffusion of Mn can be promoted, and the standard deviation of the Mn concentration can be reduced. Therefore, it is preferred to perform hot rolling in a temperature range of 850 to 1100°C to reduce the plate thickness by more than 90%.
[0184] It should be noted that the thickness reduction in the temperature range of 850 to 1100° C. is defined as the plate thickness before the initial rolling in the rolling in this temperature range being t 0 The exit plate thickness after rolling in the final stage of rolling in this temperature range is set as t 1 When {(t 0 -t 1 ) / t 0}×100(%).
[0185] (6-3) Stress after the hot rolling in the first stage before the final stage and before the final stage: 170 kPa or more
[0186] It is preferred that the stress applied to the steel sheet after the hot rolling of the first stage before the final stage and before the final stage be set to 170 kPa or more. This can reduce the {110} <001> The number of crystal grains with the crystal orientation {110} <001> Since it is a crystal orientation that is difficult to recrystallize, by suppressing the formation of this crystal orientation, the recrystallization brought about by the final stage of pressing can be effectively promoted. As a result, the banded structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value is increased. When the stress applied to the steel sheet is less than 170 kPa, it may not be possible to achieve an E value of 10.7 or more. The stress applied to the steel sheet is more preferably 190 kPa or more. The stress applied to the steel sheet can be controlled by adjusting the roller rotation speed in the tandem rolling.
[0187] (6-4) Reduction ratio in the final stage of hot rolling: 8% or more, hot rolling finishing temperature Tf: 900°C or more and less than 1010°C
[0188] Preferably, the reduction rate in the final section of hot rolling is set to 8% or more, and the hot rolling finishing temperature Tf is set to 900°C or more. By setting the reduction rate in the final section of hot rolling to 8% or more, the recrystallization brought about by the reduction in the final section can be promoted. As a result, the banded structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value is increased. By setting the hot rolling finishing temperature Tf to 900°C or more, the excessive increase in the number of ferrite nucleation sites in austenite can be suppressed. As a result, the formation of ferrite in the final structure (the metal structure of the hot-rolled steel sheet after manufacture) can be suppressed, and a high-strength hot-rolled steel sheet can be obtained. In addition, by setting Tf to less than 1010°C, the coarsening of the austenite grain size can be suppressed, and the periodicity of the metal structure can be reduced to set the E value to 10.7 or more.
[0189] (6-5) Stress after hot rolling and before the steel plate is cooled to 800°C: less than 200 kPa
[0190] The stress applied to the steel plate after rolling in the final stage of hot rolling and before the steel plate is cooled to 800°C is preferably set to less than 200 kPa. By setting the stress applied to the steel plate to less than 200 kPa, the recrystallization of austenite preferentially progresses along the rolling direction, and the increase in the periodicity of the metal structure can be suppressed. As a result, the E value can be set to 10.7 or more. The stress applied to the steel plate is more preferably less than 180 MPa.
[0191] (6-6) After cooling to a temperature range below the hot rolling completion temperature Tf-50°C within 1 second after the hot rolling is completed, accelerated cooling is performed at an average cooling rate of 50°C / second or more to a temperature range of 600 to 730°C.
[0192] In order to suppress the growth of austenite grains that are fine-grained by hot rolling, it is more preferable to cool by 50°C or more within 1 second after the hot rolling is completed. In order to cool to a temperature range below the hot rolling completion temperature Tf-50°C within 1 second after the hot rolling is completed, it is sufficient to perform cooling with a high average cooling rate immediately after the hot rolling is completed, such as spraying cooling water on the steel plate surface. By cooling to a temperature range below Tf-50°C within 1 second after the hot rolling is completed, the crystal grain size of the surface layer can be refined, and the bending crack resistance can be improved.
[0193] In addition, by accelerating cooling to a temperature range below 730°C at an average cooling rate of 50°C / second or more after the above cooling, the formation of ferrite and pearlite with a small amount of precipitation strengthening can be suppressed. As a result, the strength of the hot-rolled steel sheet is improved. It should be noted that the so-called average cooling rate here refers to the following value: the temperature drop of the steel plate from the start of accelerated cooling (when the steel plate is introduced into the cooling equipment) to the completion of accelerated cooling (when the steel plate is derived from the cooling equipment) divided by the required time from the start of accelerated cooling to the completion of accelerated cooling.
[0194] The upper limit of the cooling rate is not particularly specified, but if the cooling rate is increased, the cooling equipment becomes large-scale and the equipment cost becomes high. Therefore, if the equipment cost is taken into consideration, it is preferably 300°C / second or less. In addition, the cooling stop temperature of the accelerated cooling is preferably set to 600°C or more.
[0195] (6-7) Slow cooling is performed in a temperature range of 600 to 730°C for 2.0 seconds or more with an average cooling rate of less than 5°C / second.
[0196] By performing slow cooling with an average cooling rate of less than 5°C / second for more than 2.0 seconds in a temperature range of 600 to 730°C, precipitation-strengthened ferrite can be fully precipitated. Thus, the strength and ductility of the hot-rolled steel sheet can be taken into account. It should be noted that the so-called average cooling rate here refers to the following value: the temperature drop of the steel plate from the cooling stop temperature of the accelerated cooling to the stop temperature of the slow cooling divided by the time required from the stop of the accelerated cooling to the stop of the slow cooling.
[0197] The time for slow cooling is preferably 3.0 seconds or more. The upper limit of the time for slow cooling is determined by the equipment layout, but it can be set to about less than 10.0 seconds. In addition, the lower limit of the average cooling rate of slow cooling is not particularly set, but since the temperature increase without cooling will be accompanied by a large investment in equipment, it can also be set to 0°C / second or more.
[0198] (6-8) Average cooling rate to coiling temperature: 50°C / sec or more
[0199] In order to suppress the area fraction of pearlite and obtain a tensile strength of 980 MPa or more, it is preferred to set the average cooling rate from the cooling stop temperature of slow cooling to the coiling temperature to 50°C / second or more. In this way, the parent phase structure can be made hard. It should be noted that the so-called average cooling rate here refers to the following value: the temperature drop of the steel plate from the cooling stop temperature of slow cooling with an average cooling rate of less than 5°C / second to the coiling temperature divided by the time required from the stop of slow cooling with an average cooling rate of less than 5°C / second to coiling.
[0200] (6-9) Coiling temperature: above 400°C and below 600°C
[0201] The coiling temperature is set to a temperature range of 400° C. or higher and lower than 600° C. By setting the coiling temperature to this temperature range, the precipitation amount of iron carbides can be increased, and the hardness distribution in the hard phase can be improved. As a result, the I value can be reduced, and excellent shear workability can be obtained.
[0202] Example
[0203] Next, the effect of one scheme of the present invention is described more specifically through an embodiment, but the conditions in the embodiment are a conditional example adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this conditional example. As long as it does not deviate from the main purpose of the present invention and achieves the purpose of the present invention, the present invention can adopt various conditions.
[0204] Steels having the chemical compositions shown in Tables 1 and 2 were melted and continuously cast to produce slabs having a thickness of 240 to 300 mm. The obtained slabs were used to produce hot-rolled steel sheets shown in Tables 5A to 6B under the manufacturing conditions shown in Tables 3A to 4B. It should be noted that the average cooling rate of slow cooling was set to less than 5°C / sec.
[0205] The area fraction of the metal structure, E value, I value, standard deviation of Mn concentration, average crystal grain size of the surface layer, tensile strength TS and total elongation El of the obtained hot-rolled steel sheet were determined by the above-mentioned method. The obtained measurement results are shown in Tables 5A to 6B.
[0206] It should be noted that the remaining structure is one or two or more of bainite, martensite, and tempered martensite.
[0207] Evaluation method of characteristics of hot-rolled steel sheets
[0208] (1) Tensile strength characteristics
[0209] When the tensile strength TS is 980 MPa or more, the total elongation El is 12.0% or more, and the tensile strength TS×total elongation El is 15000 MPa·% or more, the hot-rolled steel sheet is judged as qualified as having excellent strength and ductility. If any one of them is not satisfied, the hot-rolled steel sheet is judged as not having excellent strength and ductility.
[0210] (2) Shear processability
[0211] The shear workability of hot-rolled steel sheets is evaluated by obtaining the shear surface ratio using a punching test. Five punching holes were made at the center of the plate width with a hole diameter of 10 mm, a clearance of 15%, and a punching speed of 3 m / s. Next, for the five punching holes, 10 end faces parallel to the rolling direction (two end faces for each punching hole) were photographed using an optical microscope. In the obtained observation photos, it can be observed Figure 1 (a) shows the end face. Figure 1 As shown in (a) and (b), collapsed edges, shear surfaces, fracture surfaces, and fins were observed at the end surfaces after punching. Figure 1 (a) is a schematic diagram of the end surface of the punched hole parallel to the rolling direction. Figure 1 (b) is a schematic diagram of the side of the punched hole. The so-called collapsed edge is an R-shaped smooth surface, the so-called shear surface is a punched end surface separated by shear deformation, the so-called fracture surface is a punched end surface separated by cracks generated near the blade tip after the shear deformation is completed, and the so-called flying fin is a surface with a protrusion extending from the lower surface of the hot-rolled steel plate. In the observation photos of 10 end surfaces obtained from 5 end surfaces, the shear surface ratio occupied by the end surface is measured, and the value obtained by dividing the minimum value of the obtained shear surface ratio (%) by the maximum value is calculated (minimum value of shear surface ratio / maximum value of shear surface ratio). When this value is 0.70 or more, it is judged as a hot-rolled steel plate with excellent shear workability and is qualified. On the other hand, when this value is less than 0.70, it is judged as an unqualified hot-rolled steel plate with poor shear workability.
[0212] It should be noted that the ratio of the shear surface to the end surface (shear surface ratio) is obtained by the following method: Figure 1As shown in (a), a straight line 1 is drawn at right angles to the upper and lower surfaces of the hot-rolled steel plate in the end surface observation photograph, and the ratio of the length d2 of the shear surface in the straight line 1 to the total of the collapsed edge length d1, the shear surface length d2, the fracture surface length d3 and the fin length d4 is calculated (= d2 / (d1+d2+d3+d4)×100).
[0213] (3) Resistance to internal cracking during bending
[0214] The bending crack resistance was evaluated by the following bending test.
[0215] A 100 mm × 30 mm strip-shaped test piece was cut out from the 1 / 2 position in the width direction of the hot-rolled steel plate to obtain a bending test piece. For both bending in which the bending ridgeline is parallel to the rolling direction (L direction) (L-axis bending) and bending in which the bending ridgeline is parallel to the direction perpendicular to the rolling direction (C direction) (C-axis bending), the bending internal cracking resistance was investigated according to JIS Z 2248:2014 (V-block 90° bending test), and the minimum bending radius without cracking was calculated. The value obtained by dividing the average value of the minimum bending radius of the L axis and the C axis by the plate thickness is set as the limit bending R / t, which is used as an index value of the bending internal cracking resistance. When R / t is 2.5 or less, it is judged to be a hot-rolled steel plate with excellent bending internal cracking resistance.
[0216] Regarding the presence or absence of cracks, the cross section of the test piece after the V-block 90° bending test was cut along a plane parallel to the bending direction and perpendicular to the plate surface, mirror polished, and then cracks were observed under an optical microscope. When the length of the crack observed on the inner side of the bend of the test piece exceeded 30 μm, it was judged that cracks were present.
[0217] The obtained results are shown in Table 6A and Table 6B.
[0218] [Table 1]
[0219]
[0220] [Table 2]
[0221]
[0222] [Table 3A]
[0223]
[0224] The underline indicates that the manufacturing conditions are not preferred.
[0225] [Table 3B]
[0226]
[0227] The underline indicates that the manufacturing conditions are not preferred.
[0228] [Table 4A]
[0229]
[0230] The underline indicates that the manufacturing conditions are not preferred.
[0231] [Table 4B]
[0232]
[0233] The underline indicates that the manufacturing conditions are not preferred.
[0234] [Table 5A]
[0235]
[0236] Underlining indicates features that are outside the scope of the present invention or are not preferred.
[0237] [Table 5B]
[0238]
[0239] Underlining indicates features that are outside the scope of the present invention or are not preferred.
[0240] [Table 6A]
[0241]
[0242] Underlining indicates features that are outside the scope of the present invention or are not preferred.
[0243] [Table 6B]
[0244]
[0245] Underlining indicates features that are outside the scope of the present invention or are not preferred.
[0246] If we observe Tables 5A to 6B, we can see that the hot-rolled steel sheets of the examples of the present invention have excellent strength, ductility and shear workability. In addition, we can see that the hot-rolled steel sheets of the examples of the present invention, whose average crystal grain size of the surface layer is less than 3.0 μm, have excellent resistance to bending cracking in addition to the above-mentioned properties.
[0247] On the other hand, it is found that the hot-rolled steel sheets of the comparative examples do not have excellent strength, ductility, or shear workability.
[0248] Industrial Applicability
[0249] According to the above-mentioned embodiment of the present invention, a hot-rolled steel sheet having excellent strength, ductility and shear workability can be provided. In addition, according to the above-mentioned preferred embodiment of the present invention, a hot-rolled steel sheet having excellent resistance to bending cracking, i.e., suppressing the occurrence of bending cracking, can be obtained while having the above-mentioned characteristics.
[0250] The hot-rolled steel sheet of the present invention is suitable as an industrial raw material used in automobile components, mechanical structural components, and even building components.
Claims
1. A hot rolled steel plate, characterized in that: The chemical composition is expressed in mass % as follows: C:0.050~0.250%、 Si: 0.05-3.00%, Mn: 1.00~4.00%, One or more of Ti, Nb and V: 0.060 to 0.500% in total, Sol.Al: 0.001~2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Cu: 0-2.00%, Cr:0~2.00%、 Mo: 0-1.00%, Ni: 0-2.00%, B:0~0.0100%、 Ca: 0~0.0200%, Mg: 0~0.0200%, REM: 0~0.1000%、 Bi: 0~0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0~0.05%, The rest is Fe and impurities. The metal structure is as follows: The retained austenite is less than 3.0%, the ferrite is more than 15.0% and less than 60.0%, and the pearlite is less than 5.0% in terms of area%. The E value representing the periodicity of the metal structure is greater than 10.7, and the I value representing the uniformity of the metal structure is less than 1.020; The standard deviation of the Mn concentration is 0.60 mass % or less, The tensile strength is above 980MPa. In the measurement of E value and I value, the shooting area of the SEM image taken to calculate the E value and I value was set to: a depth position of 1 / 4 of the plate thickness from the steel plate surface in a cross section parallel to the rolling direction and a central position in the plate width direction, In the determination of the standard deviation of the Mn concentration, after the L-section of the hot-rolled steel plate parallel to the rolling direction is mirror-polished, the center position of the steel plate in the plate width direction at a depth of 1 / 4 of the plate thickness from the surface is measured using an electron probe microanalyzer EPMA to determine the standard deviation of the Mn concentration.
2. The hot rolled steel sheet according to claim 1, characterized in that: The average crystal grain size of the surface layer is less than 3.0 μm.
3. The hot rolled steel sheet according to claim 1 or 2, characterized in that: The chemical composition contains, by mass%, one or more elements selected from the following: Cu: 0.01-2.00%, Cr:0.01~2.00%、 Mo: 0.01~1.00%, Ni: 0.02-2.00%, B:0.0001~0.0100%、 Ca: 0.0005~0.0200%, Mg: 0.0005~0.0200%, REM: 0.0005~0.1000%, and Bi: 0.0005~0.020%.
Citation Information
Patent Citations
Cold rolled steel sheet excellent in blanking property and its production
JP1998168544A
High strength automobile steel plate superior in collision safety and formability, and its manufacture
JP1999061326A
High strength steel sheet having excellent elongation and stretch-flange formability
JP2005179703A
High strength hot rolled steel sheet having excellent stamping workability and its production method
JP2005298924A
High-strength hot dip zinc plated steel sheet having excellent moldability, and method for production thereof