A method for preparing concrete and concrete
By preparing nano-covered films on the surface of the aggregate, the problems of high nanomaterial dosage and high cost are solved, the early strength and durability of concrete are improved, and both economic and performance improvements are achieved.
Patent Information
- Application Number
- CN202211703964.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The problems of high amount and high cost of nanomaterials in the prior art make it difficult to promote and apply them on a large scale in concrete.
Prepare a nano-coated film on the surface of the aggregate, and then stir the nanomaterial and dispersant in water and then perform ultrasonic dispersion to form a nanodispersion liquid, and it is coated on the aggregate by immersion, spraying, spraying or negative pressure immersion. On the surface, a nano-coated film with a thickness of 5 to 20 μm was formed.
It significantly reduces the amount of nanomaterials, improves the early strength and durability of concrete, reduces costs, and avoids the adverse effects of rust and dyed aggregates on the strength of concrete, and has the prospect of promotion and application.
Smart Images

Figure CN116119958B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydraulic concrete, and in particular relates to a preparation method of concrete and the concrete. Background Art
[0002] Nanomaterials have attracted wide attention due to a series of special effects such as small size effect, surface and interface effect, quantum effect, macroscopic quantum tunneling effect, etc., and are known as "the most promising materials in the 21st century". In the 1990s, nanomaterials began to be used in the field of cement concrete. The direct addition method is the most widely used method, that is, adding nanomaterials (nanopowders or nanodispersions) directly during the concrete mixing process. Concrete with nanomaterials exhibits better mechanical properties and durability: compressive strength and splitting strength are improved, and durability is significantly improved. However, since nanomaterials are easy to agglomerate and difficult to disperse in concrete, coupled with high cost, the direct addition method requires a high amount of nanomaterials, resulting in a significant increase in concrete cost (the cost of a single cubic meter of concrete increases by hundreds of yuan). Therefore, nanomaterials have not been widely used and promoted in concrete so far.
[0003] How to fully utilize and give play to the special effects of nanomaterials and develop nano application technologies that are suitable for hydraulic concrete and are both economical has become a research difficulty in the hydraulic field. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of high dosage and high cost of nanomaterials in the prior art, thereby providing a method for preparing concrete and concrete.
[0005] To this end, the present invention provides the following technical solutions.
[0006] A method for preparing concrete comprises preparing a nano coating film on a part or all of the aggregate surface, wherein the thickness of the nano coating film is 5 to 20 μm.
[0007] Furthermore, preparing the nano-coating film on the aggregate surface includes the following steps:
[0008] Step 1, preparing a nano-dispersion liquid;
[0009] Step 2, coating the nano-dispersion on the aggregate surface;
[0010] Step 3: drying to obtain aggregate with a nano-coated film on the surface.
[0011] Furthermore, the step 1 comprises: adding the nanomaterial and the dispersant into water, stirring and then performing ultrasonic dispersion to obtain a nano-dispersion liquid.
[0012] Further, the nanomaterial includes at least one of nano calcium carbonate, nano silicon dioxide, nano aluminum oxide or nano TiO2;
[0013] The dispersant includes at least one of sodium hexametaphosphate, sodium dodecylbenzene sulfonate, and polycarboxylate;
[0014] Preferably, the dispersant comprises sodium hexametaphosphate and polycarboxylate, and the mass ratio of the sodium hexametaphosphate to the polycarboxylate is (1-3): (3-1).
[0015] Exemplarily, the polycarboxylate is PEO[(CH2CH2O) n ](n=15~25).
[0016] Furthermore, step 1 satisfies at least one of the following conditions:
[0017] (1) The mass ratio of the nanomaterial to the dispersant is (8-1): (1-4);
[0018] (2) The mass percentage of the nanomaterial in the nano-dispersion liquid is 1% to 6%;
[0019] (3) The ultrasonic dispersion time is 5 to 25 minutes.
[0020] Furthermore, the step 2 comprises: coating the nano-dispersion on the aggregate surface by soaking, spraying, coating or negative pressure impregnation.
[0021] Further, the soaking includes:
[0022] Immerse the aggregate to be treated in the nanodispersion for 10-20 minutes;
[0023] Alternatively, a porous container containing the aggregate to be treated is immersed in the nano-dispersion for 1 minute, lifted up, rotated around a horizontal axis, and then immersed again, and this is repeated 10-20 times.
[0024] Furthermore, the spraying is: spraying the nano-dispersed liquid on the surface of the aggregate through a pressure-free nozzle;
[0025] For example, the spraying with a pressureless nozzle is suitable for coating thin layers of aggregate layer by layer. First, the aggregate is spread on the ground with a thickness of about 20 cm, and the pressureless nozzle is moved back and forth in a straight line to spray the nano dispersion on the surface of the aggregate until the dispersion is evenly distributed on the surface of the aggregate; then the second layer of aggregate is spread with a thickness of 20 cm, and the nano dispersion is continued to be sprayed; then the third layer of aggregate is spread with a thickness of 20 cm, and the nano dispersion is sprayed; and this is repeated until the last layer of the aggregate pile is sprayed.
[0026] The spraying is: spraying the nano-dispersed liquid on the surface of the aggregate through a pressure nozzle;
[0027] Exemplarily, pressure nozzle spraying is suitable for coating thick aggregates layer by layer, and is also suitable for in-situ coating of aggregates in fixed containers (such as a hopper with a volume of 5 cubic meters and a loading and unloading truck with a volume of no more than 10 cubic meters).
[0028] When thick layers of aggregate are coated layer by layer, the thickness of each layer of aggregate can be 40cm to 50cm, and then the nozzle moves back and forth in a straight line to spray and coat, and then the aggregate is spread to coat the next layer.
[0029] When the aggregate in a fixed container is coated in situ, the nozzle rotates while spraying, spraying the aggregate in the container at multiple angles until the surface of the aggregate is wetted by the dispersion. At the same time, the dispersion can also penetrate into the interior through the pores between the aggregates, ensuring that the deep aggregate is also coated with the nano-dispersion.
[0030] The negative pressure impregnation is: in a closed environment with a vacuum degree of 70 kPa to 10 kPa, the nano-dispersed liquid is introduced by negative pressure to achieve the impregnation of the aggregate.
[0031] Furthermore, the aggregate includes coarse aggregate and fine aggregate, and a nano-coating film is prepared on the surface of all or part of the coarse aggregate; and / or, a nano-coating film is prepared on the surface of all or part of the fine aggregate.
[0032] Concrete prepared according to the above preparation method.
[0033] The coated aggregate is dried to a saturated surface dry state by natural air drying or artificial accelerated air drying. No other treatment measures are required. The surface of the aggregate is deposited and agglomerated to form a nano-coating film with a thickness of no more than 20um.
[0034] Aggregates coated with nanofilm can be mixed and molded in the conventional way, without the need for additional processes and without interfering with the traditional molding method.
[0035] The technical solution of the present invention has the following advantages:
[0036] 1. The method for preparing concrete of the present invention comprises preparing a nano coating on a part or all of the aggregate surface, wherein the thickness of the nano coating is 5 to 20 μm.
[0037] The present invention only forms a micron-scale nano-coating film on the surface of the aggregate, and the amount of nano-material used is greatly reduced compared with the direct addition method, and the economic efficiency is obvious, and it is expected to be widely promoted and applied in the field of hydraulic concrete. The present invention forms a 5-20um thick nano-film on the surface of the aggregate, so that the microstructure of the concrete interface transition zone after forming and hardening is significantly improved, and the macroscopic performance of the concrete is significantly improved.
[0038] After adding nanomaterials, the early strength increases. Therefore, for low-heat silicate cement with relatively low early strength, the early concrete strength can be improved and the construction period can be accelerated.
[0039] Rust-stained aggregate is an aggregate with reddish-brown rust-like substances on the surface. Studies have shown that rust-like substances have an adverse effect of about 10% on the strength of concrete. For rust-stained aggregates and other aggregates whose quality is lower than the specification requirements, the method of the present invention uses nanomaterials to improve the quality of aggregates and avoid the adverse effects of rust staining, which is economically feasible and has a prospect for promotion and application.
[0040] 2. The preparation method of concrete of the present invention is to add nanometer material and dispersant into water, stir and then disperse by ultrasonic to obtain nanometer dispersion liquid. The method of the present invention can prepare nanometer dispersion liquid with uniform dispersion and long-term (5h to 10h) dispersion effect.
[0041] The dispersant comprises sodium hexametaphosphate and polycarboxylate, wherein the mass ratio of the sodium hexametaphosphate and the polycarboxylate is (1-3): (3-1). The use of the two dispersants in combination can further reduce the amount of the dispersant, achieve better dispersing effect and be more economical.
[0042] 3. In the preparation method of concrete of the present invention, the mass ratio of the nano material to the dispersant is (8-1): (1-4); the mass percentage of the nano material in the nano dispersion is 1%-6%. Within this range, a uniformly dispersed nano dispersion can be prepared, and the dispersion remains uniform within 5h-10h, providing sufficient operation time for coating the aggregate surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0044] Figure 1 is the compressive strength development curve of the concrete prepared in Example 1 and the blank concrete in Comparative Example 1;
[0045] Figure 2 is the percentage increase in compressive strength of the concrete prepared in Example 1 compared to the blank concrete;
[0046] Figure 3 is the flexural strength development curve of the concrete prepared in Example 1 and the blank concrete;
[0047] Figure 4 is the percentage increase in flexural strength of the concrete prepared in Example 1 compared to the blank concrete;
[0048] Figure 5is the compressive strength development curve of the concrete of Examples 6-8 and the blank concrete of Comparative Example 3;
[0049] Figure 6 is the splitting tensile strength development curve of the concrete of Examples 6-8 and the blank concrete of Comparative Example 3;
[0050] Figure 7 is a scanning electron microscope image of the aggregate used in the test example before the preparation of the nano-coating film;
[0051] Figure 8 This is a scanning electron microscope image of the aggregate used in the test example after the nano-coating film was prepared. DETAILED DESCRIPTION
[0052] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0053] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0054] Example 1
[0055] This embodiment provides a method for preparing concrete, comprising the following steps:
[0056] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP (sodium hexametaphosphate) and PCS (such as Sika ViscoCrete-325C) into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant (SHMP+PCS) is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0057] Step 2: Place 1 / 3 of the total mass of standard sand required for concrete into a porous container, immerse the porous container in the nano-dispersion solution for 1 minute, lift it up, rotate the container around a horizontal axis, and immerse it again, repeating the immersion process 10 times;
[0058] Step 3, drying;
[0059] Step 4: According to the standard "Cement Mortar Strength Test" (GB / T17671-1999), the standard sand coated with the nano-coating film prepared above is mixed with the remaining standard sand, standard cement and water to form a mortar specimen. The masses of the standard cement, standard sand and water are 450g, 1350g and 225g respectively.
[0060] Example 2
[0061] This embodiment provides a method for preparing concrete, comprising the following steps:
[0062] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP and PCS into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0063] Step 2, spraying the nano-dispersion liquid on the surface of standard sand (1 / 3 of the mass of all standard sand required for concrete in this embodiment), and continuously stirring the sand during the spraying process;
[0064] Step 3, drying;
[0065] Step 4: According to the standard "Cement Mortar Strength Test" (GB / T17671-1999), the standard sand coated with the nano-coating film prepared above is mixed with the remaining standard sand, standard cement and water to form a mortar specimen. The masses of the standard cement, standard sand and water are 450g, 1350g and 225g respectively.
[0066] Example 3
[0067] This embodiment provides a method for preparing concrete, comprising the following steps:
[0068] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP and PCS into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0069] Step 2: Place 1 / 3 of the total standard sand mass in a sealed bag, evacuate the bag, and then use negative pressure to introduce the nano-dispersion liquid until all the sand is soaked in the liquid, and let it stand for 5 minutes;
[0070] Step 3, drying;
[0071] Step 4: According to the standard "Cement Mortar Strength Test" (GB / T17671-1999), the standard sand coated with the nano-coating film prepared above is mixed with the remaining standard sand, standard cement and water to form a mortar specimen. The masses of the standard cement, standard sand and water are 450g, 1350g and 225g respectively.
[0072] Comparative Example 1
[0073] According to the standard "Cement Mortar Strength Test" (GB / T17671-1999), standard sand, reference cement and water are mixed to form mortar specimens. The masses of reference cement, standard sand and water are 450g, 1350g and 225g respectively.
[0074] The compressive and flexural strength tests of the mortar specimens were carried out at the specified age. The compressive strength and flexural strength test results are shown in Figure 1-Figure 5 .
[0075] Depend on Figure 1-Figure 4 It can be seen that after the sand surface is coated with 6% concentration of nano-dispersion, the compressive strength of the mortar specimens at the ages of 3d, 7d, 14d, and 28d is improved by 38.2%, 36.3%, 30.2%, and 28.9% respectively compared with the blank group of Comparative Example 1, and the flexural strength is increased by 26.9%, 8.6%, 17.1%, and 18.3% respectively; regardless of compressive strength or flexural strength, the strength improvement effect at the age of 3d is the most obvious.
[0076] Example 4
[0077] This embodiment provides a method for preparing concrete, comprising the following steps:
[0078] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP and PCS into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0079] Step 2: Put all the medium stones (particle size 20mm-40mm, rust-free aggregate) into a porous container, immerse the porous container in the nano dispersion for 1 minute, lift it up, rotate the container around the horizontal axis, and immerse it again, and repeat the immersion 10 times;
[0080] Step 3, drying;
[0081] Step 4: Mix the nano-coated medium stone with other raw materials according to the standard "Testing Procedures for Hydraulic Concrete" (SL352-2006). The mixing ratio is shown in Table 1.
[0082] Table 1 Raw material ratio of this embodiment (parts by mass)
[0083]
[0084] Example 5
[0085] This embodiment provides a method for preparing concrete, comprising the following steps:
[0086] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP and PCS into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0087] Step 2: Place all the medium stones (particle size 20mm-40mm, rust-free aggregate) in a sealed bag, evacuate the bag, and then use negative pressure to introduce the nano-dispersion liquid until the medium stones are soaked in the liquid, and let it stand for 5 minutes;
[0088] Step 3, drying;
[0089] Step 4: Mix the nano-coated medium stone prepared above with other raw materials according to the standard "Testing Procedures for Hydraulic Concrete" (SL352-2006). The mixing ratio is the same as that of Example 4.
[0090] Comparative Example 2
[0091] The raw materials were mixed according to the standard "Test Procedure for Hydraulic Concrete" (SL352-2006), and the raw material mix ratio was the same as that in Example 4.
[0092] Examples 4, 5, and Comparative Example 2 are non-rusted aggregate groups. After the prepared concrete is cured to the corresponding age, the compressive and splitting tensile strength tests of the concrete specimens are carried out in accordance with the "Test Code for Hydraulic Concrete" (SL352-2020).
[0093] Compared with the compressive strength of the blank group of concrete without rust dyeing in comparative example 2, the 7d compressive strength of Example 4 and Example 5 increased by 6.0% and 11.3% respectively. For the rust-free aggregate, the 7d compressive strength was significantly improved after the aggregate nano-coating.
[0094] Table 2 Effect of improving splitting strength of the rust-free dyeing group (compared with the blank group of comparative example 2)
[0095] Age 7d 28d 90d Example 4 5.26% 5.19% 9.09% Example 5 7.02% 6.49% 12.61%
[0096] As shown in Table 2, compared with the splitting tensile strength of the blank group concrete without rust-stained aggregate, the splitting tensile strength of Example 4 and Example 5 at 7d, 28d and 90d is greatly improved. For the rust-free aggregate, the nano-coating of the aggregate has a significant effect on improving the splitting tensile strength.
[0097] In summary, for rust-free aggregates, after nano-coating of the aggregate, the 7d compressive strength of the obtained concrete is significantly improved, and the splitting tensile strength at 7d, 28d and 90d is significantly improved. Nano-coating has a significant effect on improving the splitting tensile strength.
[0098] Example 6
[0099] This embodiment is basically the same as embodiment 4, except that the small stones and medium stones in this embodiment are all rust-stained aggregates.
[0100] Example 7
[0101] This embodiment provides a method for preparing concrete, comprising the following steps:
[0102] Step 1, prepare nano-dispersion liquid: add nano-silicon dioxide, dispersant SHMP and PCS into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion liquid with a nano-silicon dioxide mass concentration of 6%. The mass ratio of nano-silicon dioxide: dispersant is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0103] Step 2, spray the nano-dispersion liquid on the surface of the medium stone (particle size 20mm-40mm, rust-stained aggregate), and the sand is continuously stirred during the spraying process;
[0104] Step 3, drying;
[0105] Step 4: Mix the prepared nano-coated medium stone with other raw materials according to the standard "Testing Procedures for Hydraulic Concrete" (SL352-2006). The mixing ratio is the same as that of Example 4. In this example, the small stone and the medium stone are rust-stained aggregates.
[0106] Example 8
[0107] This embodiment is basically the same as Embodiment 5, except that the small stones and medium stones in this embodiment are rust-stained aggregates.
[0108] Examples 6-8 are the development curves of compressive strength and splitting tensile strength of concrete with rust-stained aggregate. Figure 5 , Figure 6 .
[0109] Comparative Example 3
[0110] This comparative example is substantially the same as comparative example 2, except that the small stones and medium stones in this comparative example are rust-stained aggregates.
[0111] Table 3 Strength improvement effect
[0112]
[0113] After nano-coating of rust-stained aggregate, the early compressive strength and splitting tensile strength are significantly improved compared with non-rust-stained aggregate. The 7d compressive strength is increased by up to 16%, and the 7d splitting tensile strength is increased by up to 22%; the compressive strength at 28d age can be increased by up to 8.8%; the splitting tensile strength at 90d age can still be increased by up to 9.8%.
[0114] To sum up, for rust-stained aggregate, when the aggregate is coated with nanomaterials, its early compressive strength and splitting tensile strength are significantly improved; if all aggregates are nano-coated, the improvement effect of mechanical properties is expected to be more significant. Therefore, this method can provide an economically feasible technical approach for improving the quality of rust-stained aggregate.
[0115] Test example
[0116] Preparation of nano-dispersion: Add nano-silica, dispersant SHMP (sodium hexametaphosphate) and PCS (such as Sika ViscoCrete-325C) into water, stir mechanically for 5 minutes and then disperse ultrasonically for 20 minutes to obtain a nano-dispersion with a nano-silica mass concentration of 6%. The mass ratio of nano-silica: dispersant (SHMP + PCS) is 6:1, and the mass ratio of SHMP: PCS is 1:1.
[0117] The coarse aggregate stones were immersed in the above nano-dispersion solution for 10 minutes, and then one was selected for surface morphology observation after drying.
[0118] The surface of the coarse aggregate stone before and after nano-coating was observed by scanning electron microscope. Figure 7 , Figure 8 . Figure 7 , Figure 8 The surface of the aggregate before and after nano-coating shows a coating film formed by nanoparticles. This nano-coating film improves the transition zone of the concrete after mixing and molding, and thus improves the early mechanical properties and durability of the concrete.
[0119] Aggregate nano-coating technology is effective in improving aggregate quality and enhancing the mechanical properties of concrete, and compared with the traditional direct addition method of applying nanomaterials, it has broad prospects for promotion and application.
[0120] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing concrete, characterized in that: Preparing a nano-coating film on part or all of the aggregate surface, wherein the thickness of the nano-coating film is 5 to 20 μm; The preparation of nano-coating film on the aggregate surface includes the following steps: Step 1, preparing a nano-dispersion liquid; Step 2, coating the nano-dispersion on the surface of the aggregate; Step 3, drying to obtain aggregate with a nano-coated film on the surface; The step 1 comprises: adding the nano material and the dispersant into water, stirring and then performing ultrasonic dispersion to obtain a nano dispersion; The dispersant comprises sodium hexametaphosphate and polycarboxylate, and the mass ratio of the sodium hexametaphosphate to the polycarboxylate is (1-3): (3-1); The mass ratio of the nano material to the dispersant is (8-1): (1-4); The mass percentage of the nano material in the nano dispersion is 1% to 6%.
2. The method for preparing concrete according to claim 1, characterized in that: The nano material includes at least one of nano calcium carbonate, nano silicon dioxide, nano aluminum oxide or nano TiO2.
3. The method for preparing concrete according to claim 1 or 2, characterized in that: The ultrasonic dispersion time is 5 to 25 minutes.
4. The method for preparing concrete according to claim 1, characterized in that: The step 2 comprises: coating the nano-dispersion on the aggregate surface by soaking, spraying, coating or negative pressure impregnation.
5. The method for preparing concrete according to claim 4, characterized in that: The soaking comprises: Immerse the aggregate to be treated in the nanodispersion for 10-20 minutes; Alternatively, a porous container containing the aggregate to be treated is immersed in the nano-dispersion for 1 minute, lifted up, rotated around a horizontal axis, and then immersed again, and this is repeated 10-20 times.
6. The method for preparing concrete according to claim 4, characterized in that: The spraying is: spraying the nano-dispersed liquid on the surface of the aggregate through a pressure-free nozzle; The spraying is: spraying the nano-dispersed liquid on the surface of the aggregate through a pressure nozzle; The negative pressure impregnation is: in a vacuum closed environment, using negative pressure to introduce the nano dispersion and achieve the impregnation of the aggregate.
7. The method for preparing concrete according to claim 1 or 2, characterized in that: The aggregate includes coarse aggregate and fine aggregate, and a nano-coating film is prepared on the surface of all or part of the coarse aggregate; and / or, a nano-coating film is prepared on the surface of all or part of the fine aggregate.
8. Concrete obtained according to the preparation method according to any one of claims 1 to 7.