Method for preparing spherical uranium nitride particles and uranium nitride particles
By mixing uranyl nitrate solution with urea and other additives, dispersing into balls and solidifying, combined with the roasting, carbonization and nitriding steps of an atmosphere furnace, the temperature sensitivity and temperature sensitivity of the production of uranium nitride spherical particles in the existing technology are solved. The problem of large-scale production has been solved, and the efficient preparation of uranium nitride spherical particles with uniform composition and controllable size has been achieved.
Patent Information
- Application Number
- CN202310189644.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-23
AI Technical Summary
In the existing technology, the internal gel process is sensitive to temperature, making it difficult to achieve large-scale production of uranium nitride spherical particles, and there is a lack of patent reports on UN spherical particle fuel in China.
A sol is formed by mixing a less-acid uranyl nitrate solution with urea, adding ammonium nitrate and carbon source, and then mixing it with polyvinyl alcohol and tetrahydroconol. It is dispersed into balls and pre-cured, and then fully reacted, cured, and aged in ammonia water. Then, it is finally roasted, carbonized and nitrided in an atmosphere furnace to obtain uranium nitride spherical particles.
This method does not require cooling for stability, the carbon is evenly dispersed in the glue liquid, and the amount of waste liquid is small. The uranium nitride spherical particles obtained have uniform composition, controllable size, and adjustable density. The process is intensive and easy to produce on a large scale.
Smart Images

Figure CN116120071B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nitride ceramics, and in particular to a method for preparing spherical uranium nitride particles and the uranium nitride particles. Background Art
[0002] Uranium nitride (UN) has the advantages of high thermal conductivity and high uranium density, and is one of the important candidates for accident-tolerant fuel. Tri-isotropic fuel (TRISO) particles with UN spherical particles as the core will be both efficient and safe.
[0003] The preparation and research of UN spherical particles are mostly seen abroad, usually using the internal gel process combined with carbon thermal reduction nitridation. However, the internal gel process is sensitive to temperature, requiring the gel to be stored and dispersed at low temperatures (0-4°C), which has high requirements for equipment and operation, and is not conducive to large-scale application. At present, domestic patents on UN fuel are concentrated on the preparation of powders and pellets, and there are few reports specifically on UN spherical particle fuels. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent.
[0005] In the first aspect of the present invention, a method for preparing spherical uranium nitride particles is proposed. The method comprises the following steps: step S1: mixing an acid-deficient uranyl nitrate solution with urea to form a sol; step S2: adding ammonium nitrate and a carbon source to the sol, and stirring to obtain a uniformly dispersed dispersion, then adding an additive to the dispersion, and stirring to obtain a pre-dispersed gel solution, wherein the additive comprises a polyvinyl alcohol solution and tetrahydroconol; step S3: dispersing the pre-dispersed gel solution into balls, and dropping it through an ammonia zone for pre-curing treatment to obtain spherical particles with a gelled and hardened outer layer; step S4: placing the spherical particles in ammonia water, performing a sufficient reaction, curing and aging treatment to obtain gel particles; step S5: washing and drying the gel particles in sequence; step S6: placing the dried gel particles in an atmosphere furnace for roasting, carbonization and nitridation treatment in sequence to obtain the uranium nitride particles. Therefore, the colloid in this method does not need to be cooled and is stable at room temperature. The carbon is evenly dispersed in the colloid, the amount of waste liquid is small, and the obtained uranium nitride spherical particles have uniform composition, controllable size, and adjustable density. The process flow is intensive and easy to realize large-scale production.
[0006] According to an embodiment of the present invention, before the dispersion, the glue satisfies at least one of the following conditions: the molar ratio of carbon atoms to uranium atoms is 2.0-4.0; the molar ratio of the ammonium nitrate to the uranium atoms is 0.5-2.5; the molar ratio of the polyvinyl alcohol to the uranium atoms is 0.1-1.0; the molar ratio of the tetrahydroconol to the uranium atoms is 1.0-3.0; the concentration of the under-acidified uranyl nitrate solution is 1.8-2.5 mol / L; the molar ratio of the urea to the uranium atoms is 1.8-2.6; the concentration of the polyvinyl alcohol solution is 5wt%-15wt%.
[0007] According to an embodiment of the present invention, the pre-curing treatment includes: placing the pre-dispersed glue liquid into a storage tank with a predetermined air pressure and conveying it to the nozzle of the storage tank; the pre-dispersed glue liquid is jet-segmented under vibration conditions, freely falls under the action of gravity, and sphericalizes in the air zone to obtain spherical droplets; the spherical droplets fall into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with the outer layer gelled and hardened.
[0008] According to an embodiment of the present invention, the spheronization and curing process satisfies at least one of the following conditions: the predetermined air pressure is 0.1-1.0 MPa; the inner diameter of the nozzle is 0.2-1.5 mm; the aspect ratio of the nozzle is greater than or equal to 15; the flow rate of the glue before dispersion is 15.0-100.0 g / min; the height of the air zone is 40-150 mm; the height of the ammonia zone is 100-500 mm; the ammonia flow rate of the ammonia zone is 0.2-1.5 L / h.
[0009] According to an embodiment of the present invention, the calcination treatment includes: in a protective gas, the temperature in the atmosphere furnace is increased to 140°C~180°C at a heating rate of less than or equal to 2°C / min, and the temperature is kept warm for 1~4 hours; in the protective gas, the temperature in the atmosphere furnace is increased to 280°C~350°C at a heating rate of less than or equal to 2°C / min, and the temperature is kept warm for 1~4 hours; in the protective gas, the temperature in the atmosphere furnace is increased to 450°C~500°C at a heating rate of less than or equal to 2°C / min, and the temperature is kept warm for 1~4 hours; in the protective gas, the temperature in the atmosphere furnace is increased to 580°C~620°C at a heating rate of less than or equal to 2°C / min, and the temperature is kept warm for 1~4 hours, to obtain calcined particles.
[0010] According to an embodiment of the present invention, the carbonization treatment includes: allowing the roasted particles to be placed in the protective gas, raising the temperature in the atmosphere furnace to 1400° C. to 1500° C. at a heating rate of less than or equal to 10° C. / min, and maintaining the temperature for 2 to 6 hours to obtain uranium carbide particles.
[0011] According to an embodiment of the present invention, the nitriding treatment comprises: placing the uranium carbide particles in a nitrogen gas, raising the temperature in the atmosphere furnace to 1500° C. to 2000° C. at a heating rate of less than or equal to 10° C. / min, and maintaining the temperature for 3 to 15 hours to obtain the uranium nitride particles.
[0012] According to an embodiment of the present invention, the nitrogen flow rate in the nitriding treatment is 0.1 L / min·g(U) to 5.0 L / min·g(U).
[0013] According to an embodiment of the present invention, during the nitriding treatment, an auxiliary gas is introduced into the atmosphere furnace, the auxiliary gas includes hydrogen, and the proportion of the hydrogen is 4% to 100%.
[0014] According to an embodiment of the present invention, in the calcining process, the carbonization process and the nitriding process, the gel particles are arranged in a single layer in the atmosphere furnace.
[0015] According to an embodiment of the present invention, during the carbonization treatment and the nitridation treatment, the vacuum degree of the atmosphere furnace is less than or equal to 1×10 -1 Pa; during the calcination process, the gas pressure of the atmosphere furnace is 0.1 kPa to 0.5 kPa.
[0016] According to an embodiment of the present invention, before the calcination treatment, the gel particles are further pretreated, and the pretreatment includes: heating the gel particles to 200°C to 500°C at a heating rate of 0.25°C to 2°C / min in an air atmosphere, and keeping the temperature for 1 to 3 hours.
[0017] According to an embodiment of the present invention, in the aging treatment, the concentration of the ammonia water is 4 to 12 mol / L, the aging temperature is 30 to 80° C., and the aging time is 12 to 36 hours.
[0018] According to an embodiment of the present invention, the gel particles are washed with deionized water at a water temperature of 30 to 80° C., a volume ratio of the deionized water to the gel particles of 1 to 2.5, and a conductivity of the washing liquid after washing of less than or equal to 50 μS·m -1 .
[0019] According to an embodiment of the present invention, the washed gel particles are placed in a drying box for drying, and the drying satisfies at least one of the following conditions: the gel particles are arranged in a single layer in the drying box; the drying temperature is 40 to 80°C, and the drying time is greater than or equal to 6 hours; the vacuum degree of the drying box during the drying is 0 to 0.1 MPa.
[0020] In another aspect of the present invention, an embodiment provides a uranium nitride particle, which is prepared by the above method. Thus, the obtained spherical uranium nitride particles have uniform composition, controllable size and adjustable density. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0022] Figure 1 is a flow chart of a method for preparing spherical uranium nitride particles according to one embodiment of the present invention;
[0023] Figure 2 An optical photograph of spherical uranium nitride particles according to Example 1 of the present invention;
[0024] Figure 3 The figure is an X-ray diffraction pattern of spherical uranium nitride particles according to Example 1 of the present invention. DETAILED DESCRIPTION
[0025] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0026] The method for preparing spherical uranium nitride particles and the uranium nitride particles according to the embodiment of the present invention will be described below with reference to the accompanying drawings. First, the method for preparing spherical uranium nitride particles will be described with reference to the accompanying drawings.
[0027] like Figure 1 As shown, the method comprises the following steps:
[0028] Step S1: mixing an under-acidified uranyl nitrate solution with urea to form a sol.
[0029] According to an embodiment of the present invention, a specific method for forming a sol may include: mixing a certain concentration of under-acidified uranyl nitrate solution with urea at an ambient temperature of 10 to 35°C, and hydrolyzing and condensing the mixed solution of under-acidified uranyl nitrate and urea at a temperature of 0 to 95°C, and uranyl ions and urea are complexed to form a stable sol. Thus, a stable sol can be obtained by adopting the above-mentioned formation method. In addition, in some embodiments, the specific concentration of the under-acidified uranyl nitrate solution can be 1.8 to 2.5 mol / L, so that the under-acidified uranyl nitrate can be complexed with the components of urea, thereby improving the utilization rate of the raw materials and ensuring the stability of the formed sol.
[0030] According to an embodiment of the present invention, the molar ratio of urea to uranium atoms is 1.8 to 2.6, for example, the molar ratio of urea to uranium atoms is 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5 or 2.6. Thus, the above ratio of urea to uranium atoms can effectively ensure that urea and under-acid uranyl nitrate fully undergo complexation reaction, thereby ensuring high utilization rate of raw materials.
[0031] There are no special requirements for the specific preparation method of under-acid uranyl nitrate, and those skilled in the art can flexibly select it according to existing technical means, and no restriction is imposed here.
[0032] Step S2: adding ammonium nitrate and a carbon source to the sol, and stirring to obtain a uniformly dispersed dispersion, then adding an additive to the dispersion, and stirring to obtain a pre-dispersed sol, wherein the additive includes a polyvinyl alcohol solution and tetrahydroconol.
[0033] In some embodiments, ammonium nitrate and a carbon source can be added to the sol prepared in step S1 at an ambient temperature of 10 to 35°C, and a stirring paddle and an ultrasonic dispersion device are used to fully stir and disperse for 20 to 100 minutes to obtain a uniformly dispersed dispersion, and then an auxiliary agent is added to the dispersion, and stirring and ultrasonic dispersion are continued to be uniform, and the dispersion is allowed to stand for 0.1 to 5 hours to obtain a pre-dispersed gel solution. Thus, by mixing the above method, the sol can be fully mixed with ammonium nitrate and a carbon source; and before mixing with the auxiliary agent, the sol is pre-mixed with ammonium nitrate and a carbon source to better ensure the uniformity of the carbon source dispersion; if the sol is mixed with ammonium nitrate, a carbon source and an auxiliary agent at the same time, the uniformity of the carbon source dispersion in the pre-dispersed gel solution will be relatively reduced relative to the above-mentioned mixing step of the present invention.
[0034] There is no special requirement for the specific type of carbon source, and those skilled in the art can flexibly select it according to the actual situation, as long as it can meet the use requirements of the process of the present invention. In some embodiments, the carbon source includes but is not limited to at least one of carbon powder and fructose.
[0035] Furthermore, the additive polyvinyl alcohol is mainly used to improve the rigidity and compatibility of the glue solution before dispersion, and secondly, to adjust the viscosity of the glue solution before dispersion; the auxiliary agent tetrahydrofurfuryl alcohol is used to adjust the surface tension of the glue solution before dispersion. The above two additives can be evenly mixed with the sol and the carbon source, and no adverse phenomena such as agglomeration will occur. The effect of the polyvinyl alcohol solution on improving rigidity and compatibility and the adjustability of the surface tension of tetrahydrofurfuryl alcohol are both good, which can ensure that a lower dosage can achieve a better use effect. Furthermore, the concentration of the polyvinyl alcohol solution in the glue solution before dispersion can be 5wt% to 15wt%, such as 5wt%, 7wt%, 9wt%, 10wt%, 11wt%, 13wt%, 15wt%, and the polyvinyl alcohol solution of the above concentration has good rigidity and compatibility improvement performance.
[0036] In some embodiments, the molar ratio of carbon atoms (derived from the carbon source) to uranium atoms (derived from the under-acidified uranyl nitrate) is 2.0-4.0, such as 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, etc.; the molar ratio of ammonium nitrate to uranium atoms is 0.5-2.5, such as 0.5, 0.8, 1.0, 1.3, 1.5, 1.8, 2.0, 2. 2, 2.5, etc.; the molar ratio of polyvinyl alcohol to uranium atoms is 0.1-1.0, such as 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, etc.; the molar ratio of tetrahydroconol to uranium atoms is 1.0-3.0, such as 1.0, 1.2, 1.5, 1.7, 1.9, 2.0, 2.2, 2.4, 2.5, 2.7, 3.0, etc. Under the above parameter conditions, a stable pre-dispersion gel solution can be obtained, and the dispersion uniformity of each component in the pre-dispersion gel solution is guaranteed, and the sufficiency of the subsequent reaction is guaranteed, so as to avoid excessive or low use of a certain raw material, which ultimately affects the yield of uranium nitride. It can be seen that the amounts of the above-mentioned raw materials such as under-acid uranyl nitrate, urea, ammonium nitrate, carbon source, PVA and 4-HF of the present invention are matched and restrained with each other, and uranium nitride with higher yield and better quality is prepared under the condition that the above-mentioned multiple parameters are coordinated with each other.
[0037] Step S3: The pre-dispersed glue liquid is dispersed into balls, and then falls through an ammonia gas zone for pre-curing treatment to obtain spherical particles with a gelled and hardened outer layer.
[0038] According to some embodiments of the present invention, a specific method for preparing gel particles (the ambient temperature of the process is 10-35° C.) may be:
[0039] T1: Place the pre-dispersed glue liquid into a storage tank with a predetermined air pressure and transport it to the nozzle of the storage tank. In this step, under the condition of a predetermined air pressure of 0.1-1.0Mpa (such as 0.1Mpa, 0.2Mpa, 0.3Mpa, 0.4Mpa, 0.5Mpa, 0.6Mpa, 0.7Mpa, 0.8Mpa, 0.9Mpa, 1.0Mpa), it is transported to the dispersing nozzle through a pipeline. The predetermined air pressure can ensure that the pre-dispersed glue liquid is transported to the nozzle in the storage tank.
[0040] Among them, the inner diameter of the nozzle is 0.2-1.5mm (for example, 0.2mm, 0.5mm, 0.8mm, 1.0mm, 1.2mm, 1.5mm). The inner diameter of the nozzle can realize the control of the diameter of the glue droplets before dispersion. If the inner diameter of the nozzle is too small, it is easy for the glue to be blocked at the nozzle before dispersion. If the inner diameter of the nozzle is too large, it is not conducive to obtaining qualified gel particles. That is, the above-mentioned nozzle inner diameter of 0.2-1.5mm is conducive to the subsequent acquisition of qualified gel particles of appropriate size, and will not cause blockage at the nozzle.
[0041] The aspect ratio of the nozzle is greater than or equal to 15 (for example, it can be 15, 17, 19, 20, 22, 24, 25, 27, 29, 30, etc.). A larger aspect ratio of the nozzle can effectively reduce the disturbance of the pre-dispersed glue during the transportation process.
[0042] The flow rate of the gel solution before dispersion is 15.0-100.0 g / min (for example, it can be 15.0 g / min, 20.0 g / min, 30.0 g / min, 40.0 g / min, 50.0 g / min, 60.0 g / min, 70.0 g / min, 80.0 g / min, 90.0 g / min, 100.0 g / min). Therefore, by changing the flow rate of the gel solution before dispersion, the diameter of the subsequent spherical particles can be effectively controlled, that is, the flow rate of the gel solution before dispersion of the present invention can help obtain gel particles of appropriate size.
[0043] T2: The pre-dispersion glue liquid is segmented under vibration conditions, falls freely under gravity, and forms balls in the air zone to obtain spherical droplets. That is, after the pre-dispersion glue liquid is ejected from the nozzle, it falls freely in the air environment (air zone) and under vibration conditions (which can be achieved by an oscillator), that is, the pre-dispersion glue liquid is sphericalized to obtain spherical droplets.
[0044] Among them, the height of the air zone (i.e. the height of the free fall) is 40 to 150 mm (such as 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, etc.), thereby, the free fall at the above height can effectively sphericalize better spherical droplets.
[0045] T3: Spherical droplets fall into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with a gelled and hardened outer layer. That is, after the pre-dispersed glue liquid is spheroidized in the air zone to form spherical droplets, the spherical droplets fall into the ammonia zone, that is, into the ammonia environment, and continue to fall freely in the ammonia environment. During the falling process, the spherical droplets are pre-cured under the action of ammonia to obtain spherical particles with a gelled and hardened outer layer.
[0046] Further, the height of the ammonia zone is 100-500 mm, such as 100 mm, 200 mm, 300 mm, 400 mm, 500 mm, and the ammonia flow rate of the ammonia zone is 0.2-1.5 L / h, such as 0.2 L / h, 0.5 L / h, 0.8 L / h, 1.0 L / h, 1.2 L / h, 1.4 L / h, 1.5 L / h. Under the above conditions, the spherical droplets can be pre-cured quickly and effectively. Among them, the height of the ammonia zone is related to the ammonia concentration, the height of the air zone, the uranium concentration in the glue, and the ammonium nitrate concentration. Those skilled in the art can flexibly adjust the specific height value of the ammonia zone according to the above-mentioned ammonia concentration, the height of the air zone, the uranium concentration in the glue, the ammonium nitrate concentration and other related parameters.
[0047] Step S4: placing the spherical particles in ammonia water for sufficient reaction, solidification and aging to obtain gel particles.
[0048] According to an embodiment of the present invention, the specific method of aging treatment can be: placing the spherical particles obtained in step S3 in ammonia water with a concentration of 4 to 12 mol / L and a temperature of 30 to 80°C (in a specific embodiment, the spherical particles with an outer layer of gelation and hardening obtained after pre-curing in the ammonia zone can be directly dropped into the ammonia water), aging treatment for 12 to 36 hours to obtain gel particles ((NH4)2U2O7). Thus, uniform and stable gel particles can be obtained by fully reacting, curing and aging in ammonia water under the above conditions.
[0049] Step S5: washing and drying the gel particles in sequence.
[0050] According to an embodiment of the present invention, the method for washing the aged gel particles may be: washing the gel particles with deionized water, the washing water temperature is 30-80°C, the volume ratio of deionized water to gel particles is controlled at 1-2.5, and washing may be performed in small amounts and multiple times until the conductivity of the washing liquid is less than or equal to 50 μS·m -1 The above washing temperature is relatively mild and will not damage the gel particles. Combined with the volume ratio of deionized water to gel particles, impurities on the surface of the gel particles can be quickly cleaned without causing the gel particles to be washed and broken due to excessive water.
[0051] According to an embodiment of the present invention, the washed gel particles can be placed in an oven, the drying temperature is 40 to 80°C, the drying time is greater than or equal to 6 hours, and the vacuum degree of the drying oven is 0 to 0.1 MPa during drying. Dry and clean gel particles can be obtained under the above conditions. More preferably, during drying, the gel particles can be arranged in a single layer in the oven so that the gel particles can roll slowly. In this way, the drying time can be shortened, and the heating during drying is more uniform, so that the gel particles will not be locally overheated.
[0052] Step S6: placing the dried gel particles in an atmosphere furnace for sequential calcination, carbonization and nitridation to obtain uranium nitride particles.
[0053] According to an embodiment of the present invention, before the calcination process, the gel particles are also pretreated, and the pretreatment includes: in an air atmosphere, the gel particles are heated to 200°C to 500°C (such as 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C) at a heating rate of 0.25°C to 2°C / min (such as 0.25°C / min, 0.5°C / min, 0.75°C / min, 1°C / min, 1.25°C / min, 1.5°C / min, 1.75°C / min, 2°C / min), and kept warm for 1 to 3 hours. Thus, through the pretreatment of the above process, impurities in the pores of the gel particles can be effectively removed to improve the quality of the uranium nitride finally formed. In some embodiments, the above pretreatment process can be completed in an atmosphere furnace or a muffle furnace, thereby facilitating the control of the heating rate and the insulation temperature and time.
[0054] Furthermore, during the calcination, carbonization and nitridation processes, the gel particles are arranged in a single layer in the atmosphere furnace. Thus, the single layer arrangement allows the gel particles to be heated evenly, preventing a small amount of gel particles from being overheated or underheated, thereby affecting the yield and quality of the uranium nitride particles.
[0055] In one embodiment of the present invention, during the calcination process, the calcination stage can be carried out in multiple stages. In some specific embodiments, the calcination process includes: in a protective gas, the temperature in the atmosphere furnace is raised to 140°C to 180°C (for example, 140°C) at a heating rate of less than or equal to 2°C / min (for example, a heating rate of 0.5°C / min, 0.8°C / min, 1.0°C / min, 1.3°C / min, 1.5°C / min, 1.8°C / min, 2°C / min). ℃, 150℃, 160℃, 170℃, 180℃), and keep warm for 1-4h; in protective gas, raise the temperature in the atmosphere furnace to 280℃~350℃ (for example, 280℃, 290℃, 300℃, 310℃) at a heating rate of less than or equal to 2℃ / min (for example, the heating rate is 0.5℃ / min, 0.8℃ / min, 1.0℃ / min, 1.3℃ / min, 1.5℃ / min, 1.8℃ / min, 2℃ / min). , 320℃, 350℃), and keep warm for 1-4h; in protective gas, raise the temperature in the atmosphere furnace to 450℃-500℃ (for example, 450℃, 460℃, 470℃, 480℃, 490℃, 500℃) at a heating rate of less than or equal to 2℃ / min (for example, the heating rate is 0.5℃ / min, 0.8℃ / min, 1.0℃ / min, 1.3℃ / min, 1.5℃ / min, 1.8℃ / min, 2℃ / min) , and keep warm for 1 to 4 hours; in a protective gas, increase the temperature in the atmosphere furnace to 580°C to 620°C (for example, 580°C, 590°C, 600°C, 610°C, 620°C) at a heating rate of less than or equal to 2°C / min (for example, the heating rate is 0.5°C / min, 0.8°C / min, 1.0°C / min, 1.3°C / min, 1.5°C / min, 1.8°C / min, 2°C / min), and keep warm for 1 to 4 hours to obtain calcined particles. The obtained calcined particles are carbon-containing UO2 calcined particles. During the calcination process, (NH4)2U2O7 gel particles are calcined into carbon-containing UO3 particles in the first two stages. UO3 particles react with carbon at a temperature of 450-620°C, and carbon-containing UO3 particles are reduced to carbon-containing UO2 particles. It can be seen that the segmented calcination and heat preservation during the calcination process can ensure the full release of residual organic matter and prevent the gel particles from cracking. The protective gas includes but is not limited to inert gases such as argon.
[0056] Furthermore, during the calcination process, the gas pressure of the atmosphere furnace is 0.1 kPa to 0.5 kPa, such as 0.1 kPa, 0.2 kPa, 0.3 kPa, 0.4 kPa, 0.5 kPa, thereby ensuring a good calcination effect.
[0057] In one embodiment of the present invention, the carbonization treatment includes: making the roasted particles in the protective gas, raising the temperature in the atmosphere furnace to 1400℃~1500℃ (such as 1400℃, 1420℃, 1440℃, 1450℃, 1460℃, 1480℃, 1500℃) at a heating rate of less than or equal to 10℃ / min (such as a heating rate of 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, 10℃ / min), and keeping the temperature for 2~6h to obtain uranium carbide particles. In the above carbonization stage, the carbon-containing UO2 particles are subjected to carbonization treatment to obtain uranium carbide particles. Wherein, the protective gas includes but is not limited to inert gases such as argon.
[0058] Furthermore, the vacuum degree of the atmosphere furnace during the carbonization treatment is less than or equal to 1×10 -1 Pa, thereby, the occurrence of side reactions during the carbonization process can be avoided.
[0059] In one embodiment of the present invention, the nitriding treatment can be gradually heated to the nitriding temperature at one time, and can also be divided into multiple stages such as heating-keeping-heating-keeping, etc. Specifically: In some specific embodiments, the nitriding treatment includes: making the uranium carbide particles in nitrogen gas, the temperature in the atmosphere furnace is raised to 1500℃~2000℃ (1500℃, 1600℃, 1700℃, 1800℃, 1900℃, 2000℃) at a heating rate of less than or equal to 10℃ / min (for example, the heating rate is 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, 10℃ / min), and the temperature is kept for 3~15h to obtain uranium nitride particles. Thus, the uranium carbide particles obtained by the carbonization treatment are fully nitrided in a nitrogen environment to obtain uranium nitride particles with better quality. In other specific embodiments, the nitriding treatment can be carried out in multiple stages. For example, the uranium carbide particles are placed in a nitrogen gas, and the temperature in the atmosphere furnace is raised to 1500°C to 1700°C at a heating rate of less than or equal to 10°C / min, and kept warm for 3 to 10 hours; then the temperature is continued to be raised to 1700°C to 2000°C at a heating rate of less than or equal to 10°C / min, and kept warm for 3 to 10 hours. In this way, uranium nitride particles with better density can be obtained.
[0060] Among them, in the nitriding treatment, the nitrogen flow rate is 0.1L / min·g(U)~5.0L / min·g(U), for example, the nitrogen flow rate is 0.1L / min·g(U), 0.5L / min·g(U), 0.8L / min·g(U), 1.0L / min·g(U), 1.3L / min·g(U), 1.5L / min·g(U), 2.0L / min·g(U), 2.5L / min·g(U), 3.0L / min·g(U), 3.5L / min·g(U), 4.0L / min·g(U), 4.5L / min·g(U), 5L / min·g(U), etc., that is, the nitrogen flow rate per gram of uranium per minute is 0.1L~5.0L. Under the above conditions, it can be ensured that the uranium carbide is fully nitrided.
[0061] Furthermore, the vacuum degree of the atmosphere furnace during the nitriding treatment is less than or equal to 1×10 -1 Pa, thereby avoiding the occurrence of side reactions during the nitriding process.
[0062] Furthermore, during nitriding sintering, an auxiliary gas may be introduced into the atmosphere furnace, the auxiliary gas including hydrogen, wherein the volume ratio of hydrogen in the auxiliary gas is 4% to 100% (e.g., 4%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%), and in some specific embodiments, during nitriding treatment, nitrogen is introduced first for nitriding treatment for a period of time, and then hydrogen is introduced into the atmosphere furnace, that is, the atmosphere furnace is a nitrogen-hydrogen mixed atmosphere, and nitriding is continued for a period of time. Thus, the addition of hydrogen can achieve the removal of carbon impurities, thereby purifying the uranium nitride particles.
[0063] According to an embodiment of the present invention, after the nitriding treatment is completed, the atmosphere furnace needs to be further cooled, and argon gas protection is used during the cooling process, and the cooling rate is less than or equal to 20°C / min. In this way, excessive temperature changes can be avoided, which may cause adverse effects on the uranium nitride particles.
[0064] In another aspect of the present invention, an embodiment provides a uranium nitride particle, which is prepared by the above method. Thus, the obtained spherical uranium nitride particles have uniform composition, controllable size and adjustable density. It can be understood by those skilled in the art that the uranium nitride has all the features and advantages of the above method for preparing uranium nitride, which will not be described in detail here.
[0065] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0066] Example 1
[0067] A method for preparing spherical uranium nitride particles comprises the following steps:
[0068] (1) 10 mL of under-acid uranyl nitrate solution (U concentration is 2.5 M) and 2.7 g of urea are measured, mixed evenly, and allowed to stand for 2 h to form a stable sol;
[0069] (2) using a stirring blade and an ultrasonic dispersion device, 1.2 g of ammonium nitrate and 0.75 g of carbon powder are uniformly dispersed in the sol prepared in step (1) to obtain a dispersion liquid, and then 4.5 g of polyvinyl alcohol and 3.5 mL of tetrahydroconol are added to the dispersion liquid, and stirring and ultrasonication are continued for 60 min to obtain a pre-dispersion sol;
[0070] The molar ratio of carbon atoms to uranium atoms is 2.48; the molar ratio of ammonium nitrate to uranium atoms is 0.6; the molar ratio of polyvinyl alcohol to uranium atoms is 0.32; the molar ratio of tetrahydroconol to uranium atoms is 1.44; the molar ratio of urea to uranium atoms is 1.8; the concentration of polyvinyl alcohol solution is 8wt%;
[0071] (3) Add the obtained pre-dispersion glue liquid into a storage tank with an air pressure of 1.0Mpa, and transport it to the dispersion nozzle through a pipeline; under the external vibration caused by the exciter, the pre-dispersion glue liquid jet is segmented, and falls freely under the action of gravity, and forms balls in the air zone to obtain spherical droplets; the spherical droplets fall from the air zone into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with a gelled and hardened outer layer; the spherical particles with a gelled and hardened outer layer fall directly from the ammonia zone into concentrated ammonia water and are aged for 24 hours. Among them, the inner diameter of the nozzle is 0.6mm; the aspect ratio of the nozzle is 20; the flow rate of the pre-dispersion glue liquid is 60g / min; the height of the air zone is 100mm; the height of the ammonia zone is 200mm; the ammonia flow rate in the ammonia zone is 0.2L / h;
[0072] (4) filtering out the aged spherical gel particles, washing them with 50 mL of deionized water for 30 min each time, for a total of 3 times, and the conductivity of the washing liquid after washing is less than 50 μS·m-1;
[0073] (5) The washed spherical particles are placed in an oven at a drying temperature of 60°C for 24 hours, and the gel particles are arranged in a single layer in the oven;
[0074] (6) The dried spherical gel particles are placed in an atmosphere furnace, and the spherical gel particles are arranged in a single layer. In an argon atmosphere, the heating rate of the atmosphere furnace is 0.5°C / min, and the temperature is raised to 180°C and kept warm for 2 hours; in an argon atmosphere, the heating rate of the atmosphere furnace is 0.5°C / min, and the temperature is raised to 350°C and kept warm for 2 hours; in an argon atmosphere, the heating rate of the atmosphere furnace is 0.5°C / min, and the temperature is raised to 500°C and kept warm for 2 hours; in an argon atmosphere, the heating rate of the atmosphere furnace is 0.5°C / min, and the temperature is raised to 500°C and kept warm for 2 hours. n, heated to 600℃ and kept warm for 2h; in argon atmosphere, the heating rate of the atmosphere furnace was 2.0℃ / min, heated to 1400℃ and kept warm for 2h; in nitrogen atmosphere, the heating rate of the atmosphere furnace was 0.5℃ / min, heated to 1500℃ and kept warm for 5h, and the flow rate of N2 was 2.0L / min·g(U); after nitriding treatment, the temperature began to drop, the atmosphere in the atmosphere furnace was changed to Ar, the cooling rate was 5℃ / min, and uranium nitride particles were obtained. The optical photos of the uranium nitride particles can be referred to Figure 2 , XRD test diagram can refer to Figure 3 ,Depend on Figure 2 It can be seen that the prepared uranium nitride particles have a better spherical shape, are more uniform in size, and have an appropriate size. Figure 3 It can be seen that the phase composition of spherical particles is UN.
[0075] Example 2
[0076] A method for preparing spherical uranium nitride particles comprises the following steps:
[0077] (1) 10 mL of under-acid uranyl nitrate solution (U concentration is 2.5 M) and 2.7 g of urea are measured, mixed evenly, and allowed to stand for 2 h to form a stable sol;
[0078] (2) using a stirring blade and an ultrasonic dispersion device, 1.2 g of ammonium nitrate and 0.84 g of carbon powder are uniformly dispersed in the sol prepared in step (1) to obtain a dispersion liquid, and then 5.0 g of polyvinyl alcohol and 3.5 mL of tetrahydroconol are added to the dispersion liquid, and stirring and ultrasonication are continued for 60 min to obtain a pre-dispersion sol;
[0079] The molar ratio of carbon atoms to uranium atoms is 2.8; the molar ratio of ammonium nitrate to uranium atoms is 0.6; the molar ratio of polyvinyl alcohol to uranium atoms is 0.36; the molar ratio of tetrahydroconol to uranium atoms is 1.44; the molar ratio of urea to uranium atoms is 1.8; the concentration of polyvinyl alcohol solution is 8wt%;
[0080] (3) Add the obtained pre-dispersion glue liquid into a storage tank with an air pressure of 1.0Mpa, and transport it to the dispersion nozzle through a pipeline; under the external vibration caused by the exciter, the pre-dispersion glue liquid jet is segmented, and falls freely under the action of gravity, and spherical in the air zone to obtain spherical droplets; the spherical droplets fall from the air zone into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with a gelled and hardened outer layer; the spherical particles with a gelled and hardened outer layer fall directly from the ammonia zone into concentrated ammonia water and age for 24 hours. Among them, the inner diameter of the nozzle is 0.6mm; the aspect ratio of the nozzle is 20; the flow rate of the pre-dispersion glue liquid is 60g / min; the height of the air zone is 100mm; the height of the ammonia zone is 200mm; the ammonia flow rate in the ammonia zone is 0.2L / h;
[0081] (4) Filter out the aged spherical gel particles and wash them with 50 mL of deionized water for 30 min each time for a total of 3 times. The conductivity of the washing liquid after washing is less than 50 μS·m -1 ;
[0082] (5) The washed spherical particles are placed in an oven at a drying temperature of 60°C for 24 hours, and the gel particles are arranged in a single layer in the oven;
[0083] (6) The dried spherical gel particles were placed in an atmosphere furnace, and the spherical gel particles were arranged in a single layer. In an argon atmosphere, the heating rate of the atmosphere furnace was 0.5℃ / min, and the temperature was raised to 180℃ and kept warm for 2h; in an air atmosphere, the heating rate of the atmosphere furnace was 0.5℃ / min, and the temperature was raised to 350℃ and kept warm for 2h; in an argon atmosphere, the heating rate of the atmosphere furnace was 0.5℃ / min, and the temperature was raised to 500℃ and kept warm for 2h; in an argon atmosphere, the heating rate of the atmosphere furnace was 0.5℃ / min, and the temperature was raised to 600℃ and kept warm for 2h. The flow rate of Ar was 2.0L / min·g(U) ; In an argon atmosphere, the heating rate of the atmosphere furnace is 2.0℃ / min, the temperature is raised to 1400℃ and kept at this temperature for 2h; in a nitrogen atmosphere, the heating rate of the atmosphere furnace is 0.5℃ / min, the temperature is raised to 1500℃ and kept at this temperature for 5h, and the flow rate of N2 is 2.0L / min·g(U); in a nitrogen atmosphere, the heating rate is 5℃ / min, the temperature is raised to 1700℃ and kept at this temperature for 5h to increase the density of spherical particles; after the nitriding treatment, the temperature begins to drop, the atmosphere in the atmosphere furnace is changed to Ar, the cooling rate is 5℃ / min, and the flow rate of Ar is 2.0L / min·g(U), and uranium nitride particles are obtained.
[0084] Example 3
[0085] A method for preparing spherical uranium nitride particles comprises the following steps:
[0086] (1) 10 mL of under-acid uranyl nitrate solution (U concentration is 2.5 M) and 2.7 g of urea are measured, mixed evenly, and allowed to stand for 2 h to form a stable sol;
[0087] (2) using a stirring blade and an ultrasonic dispersion device to uniformly disperse 0.84 g of carbon powder and 1.2 g of ammonium nitrate in the sol prepared in step (1) to obtain a dispersion liquid, then adding 5.0 g of polyvinyl alcohol and 3.5 mL of tetrahydroconol to the dispersion liquid, continuing to stir and ultrasonicate for 60 min to obtain a pre-dispersion gel solution;
[0088] The molar ratio of carbon atoms to uranium atoms is 2.8; the molar ratio of ammonium nitrate to uranium atoms is 0.6; the molar ratio of polyvinyl alcohol to uranium atoms is 0.36; the molar ratio of tetrahydroconol to uranium atoms is 1.44; the molar ratio of urea to uranium atoms is 1.8; the concentration of polyvinyl alcohol solution is 8wt%;
[0089] (3) Add the obtained pre-dispersion glue liquid into a storage tank with an air pressure of 1.0Mpa, and transport it to the dispersion nozzle through a pipeline; under the external vibration caused by the exciter, the pre-dispersion glue liquid jet is segmented, and falls freely under the action of gravity, and forms balls in the air zone to obtain spherical droplets; the spherical droplets fall from the air zone into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with a gelled and hardened outer layer; the spherical particles with a gelled and hardened outer layer fall directly from the ammonia zone into concentrated ammonia water and are aged for 24 hours. Among them, the inner diameter of the nozzle is 0.6mm; the aspect ratio of the nozzle is 20; the flow rate of the pre-dispersion glue liquid is 60g / min; the height of the air zone is 100mm; the height of the ammonia zone is 200mm; the ammonia flow rate in the ammonia zone is 0.2L / h;
[0090] (4) Filter out the aged spherical gel particles and wash them with 50 mL of deionized water for 30 min each time for a total of 3 times. The conductivity of the washing liquid after washing is less than 50 μS·m -1 ;
[0091] (5) The washed spherical particles are placed in an oven at a drying temperature of 60°C for 24 hours, and the gel particles are arranged in a single layer in the oven;
[0092] (6) The dried spherical gel particles were placed in an atmosphere furnace, and the spherical gel particles were arranged in a single layer. In an argon atmosphere, the heating rate of the atmosphere furnace was 0.5°C / min, and the temperature was raised to 180°C and kept warm for 2 h. In an air atmosphere, the heating rate of the atmosphere furnace was 0.5°C / min, and the temperature was raised to 350°C and kept warm for 2 h. In an argon atmosphere, the heating rate of the atmosphere furnace was 0.5°C / min, and the temperature was raised to 500°C and kept warm for 2 h. In an argon atmosphere, the heating rate of the atmosphere furnace was 0.5°C / min, and the temperature was raised to 600°C and kept warm for 2 h. The flow rate of Ar was 2.0 L / min·g(U); In an argon atmosphere, the heating rate of the atmosphere furnace was 2.0°C / min, heated to 1400°C and kept warm for 2h; in a nitrogen atmosphere, the heating rate of the atmosphere furnace is 0.5°C / min, heated to 1500°C and kept warm for 5h, and the flow rate of N2 is 2.0L / min·g(U); in a N2-8% H2 mixed atmosphere, the heating rate is 5°C / min, heated to 1700°C and kept warm for 5h, and the flow rate of N2-8% H2 is 2.0L / min·g(U), while increasing the density of spherical particles, C impurities are removed; after the nitriding treatment, the temperature begins to drop, the atmosphere in the atmosphere furnace is changed to Ar, the cooling rate is 5°C / min, and the flow rate of Ar is 2.0L / min·g(U), and uranium nitride particles are obtained.
[0093] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0094] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing spherical uranium nitride particles, characterized in that: The following steps are involved: S1: mixing the under-acidified uranyl nitrate solution with urea to form a sol; S2: adding ammonium nitrate and a carbon source to the sol, and stirring to obtain a uniformly dispersed dispersion, then adding an additive to the dispersion, and stirring to obtain a pre-dispersed sol, wherein the additive includes a polyvinyl alcohol solution and tetrahydroconol; S3: dispersing the pre-dispersed glue into balls, and dropping the balls through an ammonia zone for pre-curing treatment to obtain spherical particles with a gelled and hardened outer layer; S4: placing the spherical particles in ammonia water for sufficient reaction, solidification and aging to obtain gel particles; S5: washing and drying the gel particles in sequence; S6: placing the dried gel particles in an atmosphere furnace for calcination, carbonization and nitridation in sequence to obtain the uranium nitride spherical particles; In step S3, the pre-dispersed glue solution is placed in a storage tank with a predetermined air pressure and transported to the nozzle of the storage tank; The pre-dispersed glue liquid is jet-sectioned under vibration conditions, falls freely under the action of gravity, and forms balls in the air zone to obtain spherical droplets; The spherical liquid droplets fall into the ammonia zone in the ammonia environment and are pre-cured to obtain spherical particles with the outer layer gelled and hardened; Before the calcination process, the gel particles are pretreated, and the pretreatment includes: In an air atmosphere, heating the gel particles to 200°C to 500°C at a heating rate of 0.25°C to 2°C / min, and keeping the temperature for 1 to 3 hours; The molar ratio of ammonium nitrate to uranium atoms is 0.5 to 2.5; The molar ratio of urea to uranium atoms is 1.8 to 2.6; The height of the air zone is 40-150 mm; The height of the ammonia zone is 100-500 mm; The ammonia flow rate in the ammonia zone is 0.2-1.5 L / h.
2. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: Before the dispersion, the glue satisfies at least one of the following conditions: The molar ratio of carbon atoms to uranium atoms is 2.0 to 4.0; The molar ratio of the polyvinyl alcohol to the uranium atoms is 0.1 to 1.0; The molar ratio of the tetrahydroconol to the uranium atom is 1.0 to 3.0; The concentration of the under-acid uranyl nitrate solution is 1.8-2.5 mol / L; The concentration of the polyvinyl alcohol solution is 5wt%-15wt%.
3. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: The pre-curing treatment satisfies at least one of the following conditions: The predetermined air pressure is 0.1~1.0Mpa; The inner diameter of the nozzle is 0.2-1.5 mm; The aspect ratio of the nozzle is greater than or equal to 15; The flow rate of the glue solution before dispersion is 15.0~100.0g / min.
4. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: The calcination process comprises: In a protective gas, the temperature in the atmosphere furnace is raised to 140°C to 180°C at a heating rate of less than or equal to 2°C / min, and kept at this temperature for 1 to 4 hours; In the protective gas, the temperature in the atmosphere furnace is raised to 280°C to 350°C at a heating rate of less than or equal to 2°C / min, and the temperature is kept for 1 to 4 hours; In the protective gas, the temperature in the atmosphere furnace is raised to 450° C. to 500° C. at a heating rate of less than or equal to 2° C. / min, and maintained at this temperature for 1 to 4 hours; In the protective gas, the temperature in the atmosphere furnace is raised to 580° C. to 620° C. at a heating rate of less than or equal to 2° C. / min, and kept at this temperature for 1 to 4 hours to obtain calcined particles.
5. The method for preparing spherical uranium nitride particles according to claim 4, characterized in that: The carbonization treatment includes: placing the calcined particles in the protective gas, raising the temperature in the atmosphere furnace to 1400° C. to 1500° C. at a heating rate of less than or equal to 10° C. / min, and maintaining the temperature for 2 to 6 hours to obtain uranium carbide particles.
6. The method for preparing spherical uranium nitride particles according to claim 5, characterized in that: The nitriding treatment includes: placing the uranium carbide particles in nitrogen gas, raising the temperature in the atmosphere furnace to 1500° C. to 2000° C. at a heating rate of less than or equal to 10° C. / min, and keeping the temperature for 3 to 15 hours to obtain the uranium nitride particles.
7. The method for preparing spherical uranium nitride particles according to claim 6, characterized in that: The nitrogen flow rate in the nitriding treatment is 0.1 L / min•g(U)~5.0 L / min•g(U).
8. The method for preparing spherical uranium nitride particles according to claim 6, characterized in that: During the nitriding treatment, an auxiliary gas is introduced into the atmosphere furnace, wherein the auxiliary gas includes hydrogen, and the proportion of the hydrogen is 4% to 100%.
9. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: In the calcining process, the carbonization process and the nitriding process, the gel particles are arranged in a single layer in the atmosphere furnace.
10. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: In the carbonization treatment and the nitridation treatment, the vacuum degree of the atmosphere furnace is less than or equal to 1×10 -1 Pa; During the calcination process, the gas pressure of the atmosphere furnace is 0.1 kPa to 0.5 kPa.
11. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: In the aging treatment, the concentration of the ammonia water is 4-12 mol / L, the aging temperature is 30-80° C., and the aging time is 12-36 h.
12. The method for preparing spherical uranium nitride particles according to claim 1, characterized in that: The gel particles are washed with deionized water at a water temperature of 30-80°C, a volume ratio of the deionized water to the gel particles of 1-2.5, and a conductivity of the washing liquid after washing of less than or equal to 50 μS•m -1 .
13. The method for preparing spherical uranium nitride particles according to claim 12, characterized in that: The washed gel particles are placed in a drying box for drying, and the drying satisfies at least one of the following conditions: The gel particles are arranged in a single layer in the drying box; The drying temperature is 40-80°C, and the drying time is greater than or equal to 6 hours; The vacuum degree of the drying box during the drying is 0-0.1 MPa.
14. A uranium nitride particle, characterized in that: Prepared by the method according to any one of claims 1 to 13.