A method and production device for preparing ultra-high purity tellurium by zone melting
By using hydrogen atmosphere and three heaters in the tellurium ingot zone melting method, the problems of complex operation, long cycle and low impurity removal efficiency in the purification process of tellurium ingot zone are solved, and high efficiency and simplification are achieved The purified tellurium ingot purification process reaches 7N purity, meeting the purity requirements of high-end materials.
Patent Information
- Application Number
- CN202310206227.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-02
AI Technical Summary
The prior art has problems such as cumbersome operation, long production cycle, low impurity removal efficiency and high cost when preparing high-purity tellurium, which is difficult to meet the needs of industrial production.
The zone melting method is adopted to perform zone melting through an atmosphere where hydrogen or hydrogen is mixed with inert gas. Three heaters are set up along the length direction of the tellurium ingot length to control the movement rate and temperature of the melting zone, and combined with gas nitrogen exhaust and exhaust treatment to achieve tellurium ingot efficient purification.
Shorten the purification cycle, improve the removal efficiency of impurities, the product purity reaches 7N or above, and reduces the impurity content. For example, the content of impurities such as Se, Si, S, Ca can be reduced to less than 15 ppb, Fe, Cu, Zn, etc. Impurities can be reduced to below 1.0 ppb to meet the needs of high-end semiconductor materials.
Smart Images

Figure CN116121847B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and a production device for preparing high-purity tellurium, and in particular to a method and a production device for preparing ultra-high-purity tellurium. Background Art
[0002] Tellurium is a rare metal with an abundance of only 0.001 ~ 0.005 g / t in the earth's crust. Its reserves are scarce and it is a good semiconductor material. With the rapid development of semiconductors and solar energy in recent years, the demand for metallic tellurium has increased year by year. For example, CdTe is one of the most important solar cell materials. HgCdTe, Bi2Te3, PbTe, etc. are good semiconductor materials. In 2021, the world's tellurium production was 580 t, of which more than 70% was used for the preparation of high-end semiconductor and detector materials. In the fields of infrared, semiconductors, detectors, etc., the purity of metallic tellurium is required to be high, and most of them are required to reach 7N and above. In addition, the price of 4N-5N tellurium is 60-70 US dollars / kg, while the price of 7N tellurium reaches 500-600 US dollars / kg. There is a high premium for the purification of metallic tellurium.
[0003] The preparation methods of high-purity tellurium include chemical methods and physical methods. The chemical method is mainly electrolysis, and the physical method is mainly vacuum distillation, zone melting, and vertical pulling. For tellurium with a purity of 4N and below, electrolysis is generally used. For tellurium with a purity of 5N-6N, a combination of chemical and physical methods is generally used for purification. First, it is purified to 4N purity by chemical methods, and then purified to 5N-6N by vacuum distillation. For tellurium with a purity of 7N and above, 5N-6N tellurium is generally used as the raw material, and it is purified to 7N and above purity through zone melting. However, traditional zone melting has low efficiency and long cycle, which is not conducive to the industrial production of tellurium. Therefore, there is an urgent need for a short process and efficient impurity removal method for purification.
[0004] CN103183322A discloses a method for preparing high-purity tellurium. The boat used in the method is a quartz boat, which is subjected to multiple cyclic zone melting in a reducing atmosphere. Each cycle is 9-12 zone meltings, and 2-3 cycles are required. After completing one cycle, the head and tail are cut off, and the next cyclic zone melting is carried out to finally obtain 6N5 high-purity tellurium. This method has a long production cycle, cumbersome operation, and new impurities are easily introduced during the operation process, resulting in poor impurity removal effect; at the same time, its production cost is high, which is not conducive to large-scale production.
[0005] CN111924811A discloses a method for preparing ultra-high purity tellurium. First, the raw materials need to be pretreated. A quartz container with a baffle inside is used. At the same time, the raw tellurium is heated to complete melting in a reducing atmosphere. The carbon powder, oxides and other impurities in the raw tellurium are intercepted on one side of the baffle, and the other side is the tellurium after preliminary purification. Using the purified tellurium, 10-12 zone melting is carried out under double melting zone conditions to obtain 7N high-purity tellurium. By adopting the above technical solution, the tellurium product obtained has high purity, but the pretreatment of the raw materials is relatively cumbersome, the melting zone length is long, the impurity removal efficiency is low, the risk of secondary pollution during operation is relatively large, and the energy consumption is high. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method and production device for preparing ultra-high purity tellurium by zone melting with high impurity removal efficiency, simple operation, short preparation cycle and high tellurium purity.
[0007] The technical solution adopted by the present invention to solve the technical problem is as follows: a method for preparing ultra-high purity tellurium by zone melting, wherein the atmosphere of the zone melting process is a hydrogen atmosphere or a mixed atmosphere of hydrogen and an inert gas;
[0008] Three heaters are arranged in sequence along the length direction of the tellurium ingot, the heating temperature of the heaters on both sides is 630°C - 660°C, and the heating temperature of the heater in the middle is 680°C - 710°C;
[0009] The molten zone movement rate of the 1st to 3rd zone melting is controlled at 0.5-0.6 mm / min; the molten zone movement rate of the 4th to 6th zone melting is controlled at 0.3-0.4 mm / min; the molten zone movement rate of the 7th and subsequent zone melting is controlled at 0.1-0.2 mm / min.
[0010] Through the above technical solution, the operation mode of changing the melting zone movement rate is adopted to improve the removal efficiency of impurities in the tellurium zone melting process, and at the same time shorten the purification cycle. In the zone melting process, three heaters are used to coordinate temperature control to make the melting zone interface flat, improve the migration efficiency of impurities in the zone melting process, and thus effectively improve the impurity removal rate.
[0011] Preferably, before starting zone melting, nitrogen is first used to fully expel the air in the zone melting furnace, and then hydrogen is introduced. Nitrogen has an average molecular weight closer to that of air, and through the above technical solution, it can be introduced into the system to better replace the air, thereby fully expelling the residual air inside the system.
[0012] Preferably, after the zone melting is completed, the introduction of hydrogen is stopped and nitrogen is introduced until the tellurium ingot is cooled.
[0013] Preferably, the hydrogen flow rate during the zone melting process is 0.2 - 0.5 L / min.
[0014] Hydrogen is a gas participating in the reaction, and its flow rate can be adapted to the progress of the reaction in the zone melting.
[0015] Preferably, the distance between two adjacent heaters is 10-15 cm. There should be a certain distance between the heaters, but not too far away; when the distance is too close, it is equivalent to forming a large single heater as a whole, and when the distance is too far, it is equivalent to three independent heaters, and the coordinated temperature control effect of the three heaters cannot be achieved; specifically, when the distance between two adjacent heaters is too close, it is not conducive to controlling the morphology of the melt zone, and when the distance is far, the temperature control effect is poor.
[0016] Preferably, the length of the tellurium ingot is 700-800 mm; the width of the melting zone is 50-70 mm; the number of zone melting is 7-10 times, and after the zone melting is completed, 8%-12% of the head end of the tellurium ingot is cut off, and 10%-15% of the tail end is cut off, and the remaining part is the 7N ultra-high purity tellurium product. Since the distribution coefficient of most impurities in tellurium is less than 1, most impurities are enriched at the end of the tellurium rod after zone melting, so the cut length of the end of the tellurium rod should be longer than the head end of the tellurium rod. Through the above technical solution, a 7N ultra-high purity tellurium product can be obtained.
[0017] The present invention provides a production device for implementing the method for preparing ultra-high purity tellurium by zone melting, comprising a zone melting system and a control system;
[0018] The zone melting system includes three heaters, a quartz tube with sealing valves installed at both ends, and a high-purity graphite boat; the high-purity graphite boat is arranged in the quartz tube; during zone melting, the tellurium ingot is placed in the high-purity graphite boat; the heater is located near the quartz tube and is used to heat the inside of the quartz tube; the high-purity graphite boat is a container commonly used to load ingots in the zone melting technology;
[0019] The control system includes a power control system, a temperature control system, and a speed control system; the speed control system is used to control the movement of the heater.
[0020] Preferably, the control system further comprises a display screen.
[0021] Through the above technical solution, the power control system controls the opening and closing of the circuit and the output power of the heater. Through the temperature control system, the temperature change during the zone melting process can be monitored in real time. The rate control system controls the movement of the heater, thereby controlling the movement rate of the melting zone during the zone melting process. The above information can be summarized and displayed on the display screen of the control system for easy viewing.
[0022] Preferably, the rate control system includes a motor, a screw rod, and a moving trolley; the motor drives the moving trolley to move through the screw rod; the moving trolley drives the heater to move along the length direction of the quartz tube. The above technical solution is a specific solution for controlling the movement of the heater through the rate control system. Other methods that can effectively control the movement of the heater can also be used in the present invention.
[0023] Preferably, it also includes a gas purification device and an exhaust gas treatment system.
[0024] Preferably, the atmosphere gas first passes through a gas purification device and then enters the quartz tube through a pipeline. Through the above technical solution, the gas can be purified to above 7N, reaching the same level as the target product to ensure that the purity of the product is not affected.
[0025] Preferably, the gas purification device (10) is provided with a hydrogen purification column and a nitrogen purification column. By means of the above technical solution, hydrogen and nitrogen can be purified.
[0026] Preferably, the tail gas discharged from the quartz tube (2) passes through the pipeline in sequence through the 1# gas washing bottle, the 2# gas washing bottle, and the ignition device for tail gas treatment. The above technical solution can achieve tail gas treatment.
[0027] Preferably, the 1# gas washing bottle contains asbestos, and the 2# gas washing bottle contains glycerin.
[0028] Asbestos is mainly used to remove volatilized metals such as selenium and tellurium, so that the volatilized metal substances can be fully condensed and adsorbed on the asbestos material; glycerin is mainly used to absorb the highly toxic substance H2Se generated during the experiment to prevent the highly toxic substance from being discharged into the environment and endangering human health; the ignition device is used to remove the H2 that has not reacted completely during the experiment to avoid safety hazards caused by direct discharge of hydrogen.
[0029] The impurities that are difficult to remove during the tellurium zone melting process are Se, Si, S, Ca, etc. The segregation of impurities during the zone melting process depends on the concentration of impurity elements in the solid and liquid phases, among which the concentration of impurities in the solid phase is C s Its concentration in the liquid phase C l The ratio of k 0 = C s / C l) is the equilibrium distribution coefficient of the impurity. The closer the equilibrium distribution coefficient is to 1, the more difficult it is to remove the impurities during the zone melting process, such as impurities Se, Si, S, etc. The distribution coefficients of most impurities in tellurium metal are less than 1, so during the zone melting process, the impurities migrate from the solid phase to the liquid phase. During the 1st to 3rd zone melting, since the impurity concentrations in the solid and liquid phases are high at this time, the segregation process of impurities is easier to carry out. In order to improve the zone melting efficiency, a faster melting zone movement rate is adopted. After the 1st to 3rd zone melting, the impurity elements in tellurium are reduced. During the 4th to 6th zone melting, in order to achieve segregation equilibrium of impurities during the metal tellurium zone melting process, the melting zone movement rate needs to be further reduced. After 6 zone meltings, most impurities in tellurium have been well removed, except for impurities Se, S, Si, etc. whose equilibrium distribution coefficients are closer to 1. At this time, in order to achieve sufficient equilibrium between impurities in the solid and liquid phases and to allow trace impurities in the solid phase to fully migrate to the liquid phase, the melting zone movement rate needs to be further reduced in the next number of zone melting. The operation mode of changing the melting zone moving rate is adopted to improve the removal efficiency of impurities in the tellurium zone melting process and shorten the purification cycle.
[0030] The amount of impurity migration during the zone melting process depends on the interface conditions of the diffusion layer. In the process of impurities reaching segregation equilibrium, impurities in the solid phase migrate to the liquid phase at the solid-liquid interface, while impurities in the liquid phase also migrate to the solid phase. The amount of impurity migration depends on the impurity concentration at the solid-liquid interface. The impurity content in the diffusion layer directly affects the zone melting purification effect. When a single heater is used for temperature control, the diffusion layer is prone to form Figure 1 The shape shown, the diffusion layer interface is conical, and in the process of impurities reaching segregation equilibrium, there is a concentration difference between the top and bottom of the conical melting zone, which is not conducive to the removal of impurities and reduces the zone melting efficiency. When three heaters are used for coordinated temperature control, the diffusion layer interface presents a relatively flat arc, and in the process of impurities reaching segregation equilibrium, no obvious concentration difference is formed, which is conducive to the removal of impurities and improves the zone melting efficiency. Through the coordinated temperature control of the three heaters of the present invention and the control of the melting zone movement speed, the flat melting zone interface can be controlled, and the distance between the top of the interface and the bottom of the interface is controlled to be 0.5-1.5 cm.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The operation mode of changing the melting zone moving rate is adopted to improve the removal efficiency of impurities in the tellurium zone melting process and shorten the purification cycle. The impurity Se can be reduced to below 15 ppb, the impurities such as Si, S, Ca, Pb, Ag can be reduced to below 5.0 ppb, and the impurities such as Fe, Cu, Zn can be reduced to below 1.0 ppb, and the product purity reaches the 7N tellurium standard;
[0033] (2) Three heaters are used to coordinate temperature control during the zone melting process to make the melting zone interface flat, and the distance between the top and bottom of the interface is controlled to be 0.5-1.5 cm. This improves the migration efficiency of impurities during the zone melting process, thereby effectively improving the impurity removal rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a photograph of the diffusion layer interface formed when the prior art uses a single heater for temperature control.
[0035] Figure 2 This is a photograph of the diffusion layer interface formed in Example 1 of the present invention.
[0036] Figure 3 It is a schematic diagram of the structure of the production equipment for preparing ultra-high purity tellurium by zone melting according to the present invention.
[0037] Description of reference numerals:
[0038] 1-1—1# heater; 1-2—2# heater; 1-3—3# heater; 2—quartz tube; 3—tellurium ingot; 4—high-purity graphite boat; 5—melting zone; 6—sealing valve; 7—motor; 8—screw rod; 9—mobile trolley; 10—gas purification device; 10-1—hydrogen purification column; 10-2—nitrogen purification column; 11—gas inlet; 12—tail gas outlet; 13—1# washing bottle; 14—2# washing bottle; 15—ignition device; 16—control system; 16-1—temperature control system; 16-2—rate control system; 16-3—display screen; 17—power control system. DETAILED DESCRIPTION
[0039] The present invention is further described in conjunction with the embodiments and drawings. The following are only preferred embodiments of the present invention, and the present invention can be implemented in many different ways as defined and covered by the claims.
[0040] The raw materials used in the embodiments of the present invention are all obtained through conventional commercial channels. Example 1
[0041] The method for preparing ultra-high purity tellurium by zone melting in this embodiment is as follows:
[0042] Put 5.5 kg of 5N tellurium material (total length of tellurium ingot is 710 mm) into the graphite boat, then put the graphite boat into the zone furnace, seal it and check the air tightness; introduce N2 for 45 min, with the flow rate controlled at 4.0 L / min. Then introduce H2 for 30 min, with the flow rate controlled at 4.0 L / min. Then reduce the H2 flow rate to 0.2 L / min, and prepare to start melting;
[0043] Three heaters are arranged in sequence along the length direction of the tellurium ingot, with a distance of 10 cm between adjacent heaters. The heating temperatures of the 1# and 3# heaters on both sides are 640°C, and the heating temperature of the 2# heater in the middle is 705°C.
[0044] The moving rate of the molten zone during the zone melting process is controlled as follows: the moving rate of the molten zone of the 1st to 3rd zone melting is controlled at 0.6 mm / min; the moving rate of the molten zone of the 4th to 6th zone melting is controlled at 0.3 mm / min; the moving rate of the molten zone of the 7th to 8th zone melting is controlled at 0.15 mm / min;
[0045] The width of the melting zone during the zone melting process is 50 mm, and the diffusion layer interface presents a relatively flat arc shape, such as Figure 2 As shown, the distance between the top and bottom of the interface is 1.5 cm, and the number of zone melting is 8. After the zone melting is completed, the heating and DC power supply are cut off, and the H2 flow is turned off at the same time, and N2 is introduced for 45 minutes, and the flow rate is controlled to 4 L / min.
[0046] After zone melting is completed, 10% of the head end and 12% of the tail end are cut off, and the remaining part is the 7N product.
[0047] Figure 3 1 is a schematic diagram of the structure of the production equipment used in the method for preparing ultra-high purity tellurium by zone melting in this embodiment; the production device used in the present invention includes a zone melting system and a control system;
[0048] The zone melting system comprises three heaters 1-1, 1-2, and 1-3, a quartz tube 2 with sealing valves 6 installed at both ends, and a high-purity graphite boat 4; the high-purity graphite boat 4 is arranged in the quartz tube 2; when zone melting is performed, a tellurium ingot 3 is placed in the high-purity graphite boat 4; the heaters 1-1, 1-2, and 1-3 are located near the quartz tube 2 and are used to heat the inside of the quartz tube 2 so that a melting zone 5 is formed in the tellurium ingot 3; the ash content of the high-purity graphite boat 4 is below 5 ppm.
[0049] The control system 16 includes a power control system 17, a temperature control system 16-1, and a speed control system 16-2; the speed control system 16-2 is used to control the movement of the heaters 1-1, 1-2, and 1-3.
[0050] The rate control system includes a motor 7, a screw rod 8, and a moving trolley 9; the motor 7 drives the moving trolley 9 to move through the screw rod 8; the moving trolley 9 drives the heaters 1-1, 1-2, and 1-3 to move along the length direction of the quartz tube 2.
[0051] The control system 16 also includes a display screen 16 - 3 .
[0052] It also includes a gas purification device 10 and an exhaust gas treatment system.
[0053] The atmosphere gas first passes through the gas purification device 10 and then enters the quartz tube 2 through the gas inlet 11 via the pipeline.
[0054] The gas purification device 10 is provided with a hydrogen purification column 10 - 1 and a nitrogen purification column 10 - 2 .
[0055] The tail gas discharged from the quartz tube 2 leaves the quartz tube 2 from the tail gas outlet 12, passes through the pipeline in turn through the 1# gas washing bottle 13, the 2# gas washing bottle 14, and the ignition device 15 for tail gas treatment; the 1# gas washing bottle 13 contains asbestos; the 2# gas washing bottle 14 contains glycerin. Example 2
[0056] The method for preparing ultra-high purity tellurium by zone melting in this embodiment is as follows:
[0057] Load 5.8 kg of 5N tellurium material (total length of tellurium ingot is 710 mm) into the graphite boat, then load the graphite boat into the zone furnace, seal and check air tightness; introduce N2 for 50 min, with the flow rate controlled at 3.0 L / min. Then introduce H2 for 30 min, with the flow rate controlled at 4.0 L / min. Then reduce the H2 flow rate to 0.3 L / min, and prepare to start melting;
[0058] Three heaters are arranged in sequence along the length direction of the tellurium ingot, with a distance of 10 cm between adjacent heaters. The heating temperatures of the 1# and 3# heaters on both sides are 635°C, and the heating temperature of the 2# heater in the middle is 710°C.
[0059] The moving rate of the molten zone during the zone melting process is controlled as follows: the moving rate of the molten zone of the 1st to 3rd zone melting is controlled at 0.5 mm / min; the moving rate of the molten zone of the 4th to 6th zone melting is controlled at 0.3 mm / min; the moving rate of the molten zone of the 7th to 8th zone melting is controlled at 0.15 mm / min;
[0060] The width of the melting zone during the zone melting process was 50 mm, the distance between the top and bottom of the interface was 1.2 cm, and the number of zone melting was 8. After the zone melting was completed, the heating and DC power supply were cut off, the H2 flow was turned off, and N2 was introduced for 250 min, with the flow rate controlled at 3 L / min.
[0061] After zone melting is completed, 8% of the head end and 10% of the tail end are cut off, and the remaining part is the 7N product.
[0062] This embodiment uses the same production equipment as that of Embodiment 1. Example 3
[0063] The method for preparing ultra-high purity tellurium by zone melting in this embodiment is as follows:
[0064] Load 6.0 kg of 5N tellurium material (total length of tellurium ingot is 750 mm) into the graphite boat, then load the graphite boat into the zone furnace, seal and check air tightness; introduce N2 for 60 min, with the flow rate controlled at 2.0 L / min. Then introduce H2 for 35 min, with the flow rate controlled at 3.0 L / min. Then reduce the H2 flow rate to 0.4 L / min, and prepare to start melting;
[0065] Three heaters are arranged in sequence along the length direction of the tellurium ingot, with the distance between adjacent heaters being 12 cm. The heating temperatures of the 1# and 3# heaters on both sides are 650°C, and the heating temperature of the 2# heater in the middle is 700°C.
[0066] The moving rate of the molten zone during the zone melting process is controlled as follows: the moving rate of the molten zone of the 1st to 3rd zone melting is controlled at 0.6 mm / min; the moving rate of the molten zone of the 4th to 6th zone melting is controlled at 0.35 mm / min; the moving rate of the molten zone of the 7th to 8th zone melting is controlled at 0.1 mm / min;
[0067] The width of the melting zone during the zone melting process was 60 mm, the distance between the top and bottom of the interface was 0.8 cm, and the number of zone melting was 9. After the zone melting was completed, the heating and DC power supply were cut off, the H2 flow was turned off, and N2 was introduced for 60 minutes, with the flow rate controlled at 2 L / min.
[0068] After zone melting is completed, 8% of the head end and 12% of the tail end are cut off, and the remaining part is the 7N product.
[0069] This embodiment uses the same production equipment as that of Embodiment 1. Example 4
[0070] The method for preparing ultra-high purity tellurium by zone melting in this embodiment is as follows:
[0071] Put 5.0 kg 5N tellurium material (total length of tellurium ingot is 700 mm) into the graphite boat, then put the graphite boat into the zone furnace, seal and check the air tightness; introduce N2 for 45 min, with the flow rate controlled at 4.0 L / min. Then introduce H2 for 45 min, with the flow rate controlled at 2.0 L / min. Then reduce the H2 flow rate to 0.5 L / min, and prepare to start melting;
[0072] Three heaters are arranged in sequence along the length direction of the tellurium ingot, with a distance of 12 cm between adjacent heaters. The heating temperatures of the 1# and 3# heaters on both sides are 650°C, and the heating temperature of the 2# heater in the middle is 705°C.
[0073] The moving rate of the molten zone during the zone melting process is controlled as follows: the moving rate of the molten zone of the 1st to 3rd zone melting is controlled at 0.6 mm / min; the moving rate of the molten zone of the 4th to 6th zone melting is controlled at 0.4 mm / min; the moving rate of the molten zone of the 7th to 8th zone melting is controlled at 0.2 mm / min;
[0074] The melting zone width during the zone melting process was 70 mm, the distance between the top and bottom of the interface was 1.5 cm, and the number of zone melting was 10. After the zone melting was completed, the heating and DC power supply were cut off, the H2 flow was turned off, and N2 was introduced for 45 minutes, with the flow rate controlled at 4L / min.
[0075] After zone melting is completed, 8% of the head end and 10% of the tail end are cut off, and the remaining part is the 7N product.
[0076] This embodiment uses the same production equipment as that of Embodiment 1. Example 5
[0077] The method for preparing ultra-high purity tellurium by zone melting in this embodiment is as follows:
[0078] Load 7.0 kg of 5N tellurium material (total length of tellurium ingot is 800 mm) into the graphite boat, then load the graphite boat into the zone furnace, seal and check air tightness; introduce N2 for 50 min, with the flow rate controlled at 3.0 L / min. Then introduce H2 for 45 min, with the flow rate controlled at 2.0 L / min. Then reduce the H2 flow rate to 0.5 L / min, and prepare to start melting;
[0079] Three heaters are arranged in sequence along the length direction of the tellurium ingot, with a distance of 10 cm between adjacent heaters. The heating temperatures of the 1# and 3# heaters on both sides are 660°C, and the heating temperature of the 2# heater in the middle is 710°C.
[0080] The moving rate of the molten zone during the zone melting process is controlled as follows: the moving rate of the molten zone of the 1st to 3rd zone melting is controlled at 0.5 mm / min; the moving rate of the molten zone of the 4th to 6th zone melting is controlled at 0.3 mm / min; the moving rate of the molten zone of the 7th to 8th zone melting is controlled at 0.1 mm / min;
[0081] The width of the melting zone during the zone melting process was 60 mm, the distance between the top and bottom of the interface was 0.5 cm, and the number of zone melting was 7. After the zone melting was completed, the heating and DC power supply were cut off, and the H2 flow was turned off at the same time. N2 was introduced for 45 minutes, and the flow rate was controlled at 4 L / min.
[0082] After zone melting is completed, 12% of the head end and 15% of the tail end are cut off, and the remaining part is the 7N product.
[0083] This embodiment uses the same production equipment as that of Embodiment 1.
[0084] Product Testing
[0085] The GDMS analysis results of the 7N tellurium products obtained in Examples 1-5 are shown in Table 1, in ppbw.
[0086] Table 1 Statistics of ultra-high purity tellurium impurities
[0087]
[0088] It can be seen from the analysis results in Table 1 that after several times of zone melting purification, 5N tellurium meets the 7N tellurium standard. The content of impurities Si and S that are not specified in the standard can also be controlled at a low level (below 3 ppbw), which meets the needs of producing high-end infrared and semiconductor materials.
Claims
1. A method for preparing ultra-high purity tellurium by zone melting, characterized in that: The atmosphere of the zone melting process is a mixed atmosphere of hydrogen and inert gas; before starting the zone melting, nitrogen is first used to fully exhaust the air in the zone melting furnace, and then hydrogen is introduced; after the zone melting is completed, the introduction of hydrogen is stopped, and nitrogen is introduced until the tellurium ingot cools down; Three heaters are arranged in sequence along the length direction of the tellurium ingot, the heating temperature of the heaters on both sides is 630°C - 660°C, and the heating temperature of the heater in the middle is 680°C - 710°C; The molten zone movement rate of the 1st to 3rd zone melting is controlled at 0.5-0.6 mm / min; the molten zone movement rate of the 4th to 6th zone melting is controlled at 0.3-0.4 mm / min; the molten zone movement rate of the 7th and subsequent zone melting is controlled at 0.1-0.2 mm / min.
2. The method for preparing ultra-high purity tellurium by zone melting according to claim 1, characterized in that: Before starting zone melting, use nitrogen to fully expel the air in the zone melting furnace, and then introduce hydrogen; after the zone melting is completed, stop introducing hydrogen and introduce nitrogen until the tellurium ingot cools down; the hydrogen flow rate during the zone melting process is 0.2 - 0.5 L / min.
3. The method for preparing ultra-high purity tellurium by zone melting according to claim 1 or 2, characterized in that: The distance between two adjacent heaters is 10-15 cm; the length of the tellurium ingot is 700-800 mm; the width of the melting zone is 50-70 mm; the number of zone melting is 7-10 times. After the zone melting is completed, 8%-12% of the head end of the tellurium ingot is cut off, and 10%-15% of the tail end is cut off. The remaining part is the 7N ultra-high purity tellurium product.