Fiber-reinforced polyamide resin composition molded product

By adding ammonium salt and reactive resin to the fiber-reinforced polyamide resin composition, and using a twin-screw extruder for melt mixing, the problems of insufficient fiber dispersion and fluidity in the existing technology are solved, and high-impact materials are achieved. Fiber-reinforced polyamide resin composition with high strength and low water absorption, suitable for electronic equipment, home appliances and other fields.

CN116133817BActive Publication Date: 2024-10-29TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180059588.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-18
Publication Date
2024-10-29
Estimated Expiration
2041-08-18

AI Technical Summary

Technical Problem

It is difficult with the existing technology to simultaneously achieve high impact strength, excellent fiber dispersion and low water absorption in molded articles in fiber-reinforced polyamide resin compositions, especially in electronic equipment and home appliances, because of the fluidity and fiber dispersion of molded articles. Insufficient sex.

Method used

A fiber-reinforced polyamide resin composition containing carbon fibers and organic fibers is used. By adding specific ammonium salts and resins with reactive functional groups to the polyamide resin, a structure of continuous phase and dispersed phase is formed, and the structure is passed through a twin-screw extruder. Melt and knead to control the particle size and distribution of resin particles to improve fiber dispersion and fluidity of molded products.

Benefits of technology

The fiber-reinforced polyamide resin composition achieves high impact strength, excellent fiber dispersion and low water absorption. It is suitable for electronic equipment, home appliances and other fields, and improves the mechanical properties and appearance quality of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004113679020000421
    Figure BDA0004113679020000421
  • Figure BDA0004113679020000431
    Figure BDA0004113679020000431
  • Figure BDA0004113679020000441
    Figure BDA0004113679020000441
Patent Text Reader

Abstract

A fiber-reinforced polyamide resin composition molded article, characterized in that it comprises: 5 to 50 parts by weight of reinforcing fiber (A), 40 to 94.9 parts by weight of polyamide resin composition (B), and 0.1 to 10 parts by weight of ammonium salt (C) formed by aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia, wherein the weight average fiber length (Lwa1) of the reinforcing fiber (A) is 0.4 to 7 mm, the polyamide resin composition (B) is composed of a polyamide resin (B1), a resin (B2) having a reactive functional group, and a compound (B3) generated by the reaction of (B1) and (B2), and the resin (B2) is dispersed in the form of particles with a number average particle size of 10 to 1,000 nm. According to the present invention, a fiber-reinforced polyamide resin composition molded article having excellent mechanical properties (bending properties, impact resistance properties), excellent fiber dispersibility and moldability, and excellent rigidity when absorbing water can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fiber-reinforced polyamide resin composition molded article comprising a polyamide resin composition and reinforcing fibers. Background Art

[0002] The molded articles containing reinforcing fibers and polyamide resin compositions are widely used for sports goods, aerospace, and general industrial applications because they are lightweight and have excellent mechanical properties. Examples of the reinforcing fibers used in these molded articles include metal fibers such as aluminum fibers and stainless steel fibers, inorganic fibers such as silicon carbide fibers and carbon fibers, aramid fibers, polyparaphenylene benzoic acid fibers, and polyisocyanate fibers. Poly(ethylene butylene oxide) (PBO) fiber and other organic fibers.

[0003] In addition, the molded products containing reinforcing fibers and polyamide resin compositions have excellent lightness and mechanical properties, so they are represented by sports components and automobile components, and have recently been used in the fields of electronic equipment housings, home appliance exterior parts, etc. In particular, since the parts for sports use, electronic equipment housings, and home appliance use require more lightweight and thin, high fluidity during molding is required. In addition, since they are used as exterior components, good appearance quality and particularly high fiber dispersion on the surface of the molded products are required. Since the bending strength and impact resistance of the molded products when falling and impacting are further required, it is required to be formed by a molding material that can show both high appearance quality and mechanical properties, and can show high fluidity that can cope with lightweight and thinning. In addition, for parts for sports use, electronic equipment housings, and home appliance use, more lightweight and thin are required, but under normal conditions, the rigidity reduction caused by the water absorption of the molded products occurs, so it is known that the bending of the molded products occurs. Therefore, it is necessary to have a molded product that can also show rigidity when absorbing water.

[0004] As means for improving mechanical properties, proposed are: a fiber-reinforced polyamide resin composition molded product comprising carbon fibers, organic fibers and a polyamide resin composition, wherein the average fiber length of the carbon fibers and the average distance between the fiber ends, and the average fiber length of the organic fibers and the average distance between the fiber ends are within a specific range (for example, refer to Patent Document 1); and a fiber-reinforced resin composition comprising carbon fibers and a polyamide resin composition and a resin having a reactive functional group (for example, refer to Patent Document 2).

[0005] Furthermore, as a technique for improving the fluidity of a molded article during molding, a resin composition containing a dendritic polyester in a molded article has been proposed (for example, see Patent Document 3).

[0006] Furthermore, as a technique for suppressing the water absorption of a molded article, a resin composition containing a polyolefin resin or an aromatic polyamide in a molded article has been proposed (for example, refer to Patent Documents 4 and 5).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2014 / 098103

[0010] Patent Document 2: International Publication No. 2010 / 107022

[0011] Patent Document 3: Japanese Patent Application Publication No. 2013-249363

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 11-140237

[0013] Patent Document 5: Japanese Patent Application Publication No. 2019-151712 Summary of the invention

[0014] Problems to be solved by the invention

[0015] Regarding the molded products obtained by the techniques of Patent Documents 1 and 2, it is described that organic fibers and resins having reactive functional groups are added in addition to carbon fibers to improve impact strength. In addition, Patent Document 3 describes that the flowability is improved by adding dendritic polyester to a polyamide resin composition.

[0016] Patent Document 4 discloses that a polyolefin resin is added to a polyamide resin composition to suppress the water absorption of a molded article. Patent Document 5 discloses that an aromatic polyamide resin having a low water absorption is used as a matrix resin to suppress the water absorption of a molded article.

[0017] However, regarding the molded product obtained by Patent Document 1, it is only described that the molded product exhibits high impact strength because it contains carbon fibers and organic fibers, but Patent Document 1 does not mention the fluidity and fiber dispersibility of the molded product formed from the polyamide resin composition, and the fluidity and fiber dispersibility of the obtained molded product are insufficient. In addition, regarding the molded product obtained by Patent Document 2, it is described that high impact strength can be exhibited by using a resin having a reactive functional group, but the fluidity and fiber dispersibility of the molded product are also not mentioned here. In addition, the molded product obtained by the technology of Patent Document 3 is characterized by high fluidity of the molded product because it contains dendritic polyester, but the improvement of fiber dispersibility is insufficient.

[0018] Furthermore, the molded articles obtained by the techniques of Patent Documents 4 and 5 contain polyolefin resins and aromatic polyamide resins having low water absorption, and therefore are characterized by high rigidity of the molded articles when they absorb water, but improvement in fiber dispersibility is insufficient.

[0019] Thus, with the prior art, in a fiber-reinforced polyamide resin composition molded article based on a polyamide resin composition, it is not possible to obtain a fiber-reinforced polyamide resin composition molded article having excellent mechanical properties (including bending properties and impact resistance properties), excellent fiber dispersion of the molded article, and further excellent moldability (fluidity) and rigidity when absorbing water (low water absorption), and it is desired to develop such a fiber-reinforced polyamide resin composition molded article.

[0020] In view of the above problems of the prior art, the present invention aims to obtain a fiber-reinforced polyamide resin composition molded product having excellent mechanical properties (bending properties, impact resistance) and excellent fiber dispersibility and moldability, and further excellent rigidity when absorbing water, and in particular, aims to provide such a molding material.

[0021] Methods for solving problems

[0022] In order to solve the above-mentioned problems, the present invention mainly has the following configurations.

[0023] (1) A fiber-reinforced polyamide resin composition molded article, comprising: 5 to 50 parts by weight of reinforcing fibers (A), 40 to 94.9 parts by weight of a polyamide resin composition (B), and 0.1 to 10 parts by weight of an ammonium salt (C) formed from an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia, wherein the weight average fiber length (Lwa1) of the reinforcing fibers (A) is 0.4 to 7 mm, the polyamide resin composition (B) comprises a polyamide resin (B1), a resin (B2) having a reactive functional group, and a compound (B3) generated by a reaction between the polyamide resin (B1) and the resin (B2), and the resin (B2) is dispersed in the form of particles having a number average particle size of 10 to 1,000 nm.

[0024] (2) The fiber-reinforced polyamide resin composition molded article according to (1), wherein the polyamide resin (B1) contained in the polyamide resin composition (B) forms a continuous phase, the resin (B2) forms a dispersed phase, and the dispersed phase contains microparticles having a particle size of 1 to 100 nm formed from the compound (B3).

[0025] (3) The fiber-reinforced polyamide resin composition molded article according to (2), wherein the area ratio of the fine particles composed of the compound (B3) in the particles composed of the resin (B2) is 20% or more.

[0026] (4) The fiber-reinforced polyamide resin composition molded article according to any one of (1) to (3), wherein the resin (B2) is a polyamide having an amino group, a carboxyl group, a metal salt of a carboxyl group, an epoxy group, an acid anhydride group and A resin having at least one reactive functional group in an oxazoline group.

[0027] (5) The fiber-reinforced polyamide resin composition molded article according to any one of (1) to (4), wherein the resin (B2) is a polyolefin resin.

[0028] (6) The fiber-reinforced polyamide resin composition molded article according to any one of (1) to (5), wherein the reinforcing fiber (A) comprises carbon fibers (A1) and organic fibers (A2), and the amount of the carbon fibers (A1) and the organic fibers (A2) is 50 to 99 parts by weight and 1 to 50 parts by weight, respectively, relative to 100 parts by weight of the total of the carbon fibers (A1) and the organic fibers (A2).

[0029] (7) The fiber-reinforced polyamide resin composition molded article according to (6), wherein the weight average fiber length (Lwa2) of the organic fiber (A2) is 3 to 7 mm.

[0030] (8) The fiber-reinforced polyamide resin composition molded article according to any one of (1) to (7), wherein the polyamide resin (B1) is a mixture of a polyamide resin (B1a) and a polyamide resin (B1b), the polyamide resin (B1a) is selected from polyamide 6 and polyamide 66, and the polyamide resin (B1b) is one or more selected from polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 1012, and polyamide 9T, and a copolymer polyamide containing at least one of them as a constituent component.

[0031] (9) The fiber-reinforced polyamide resin composition molded article according to (8), wherein the polyamide resin (B1) is a mixture of polyamide 6 resin and polyamide 610 resin.

[0032] (10) The fiber-reinforced polyamide resin composition molded article according to (8) or (9), which has a water absorption of 3.0% or less when left in an environment of 80°C x 95% RH for 24 hours.

[0033] (11) The fiber-reinforced polyamide resin composition molded article according to any one of (6) to (10), wherein the organic fiber (A2) is at least one selected from liquid crystal polyester fibers, polyarylene sulfide fibers and fluorine fibers.

[0034] Effects of the Invention

[0035] The fiber-reinforced polyamide resin composition molded product of the present invention has a good reinforcing effect and excellent impact properties because it contains reinforcing fibers and polyamide resin compositions. In addition, the fiber-reinforced polyamide resin composition molded product of the present invention has excellent fluidity, fiber dispersibility, and mechanical properties during molding of the molded product because it contains specific ammonium salts. Further, if a specific polyamide resin mixture is used, it is possible to obtain further excellent fiber dispersibility of the molded product and excellent rigidity during water absorption.

[0036] And then, such fiber reinforced polyamide resin composition molded products are extremely useful in parts of electrical / electronic equipment, household appliances, housings, automobiles and sports applications. As electrical / electronic equipment housings and parts, it is suitable for electronic parts applications represented by electronic equipment housings such as computers, televisions, video players, DVD players, cameras, audio, connectors, loudspeakers, microphones, headsets, small motors, computer-related parts, etc. As household appliances, VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts, audio parts, audio, レーザーディスク (registered trademark), CDs, DVDs and other audio and video equipment parts, lighting parts, refrigerator parts, air conditioning parts, typewriter parts, word processor parts, etc. can be cited. In addition, as optical equipment and precision machinery related parts, office computer related parts, telephone related parts, fax machine related parts, copier related parts, binoculars, cameras, clocks, etc. can be cited.

[0037] As automobile parts and vehicle-related parts, door mats, pillars, armrest boxes, various motor housings, roof racks, fenders, decorative parts, bumpers, door panels, roof panels, covers, trunk lids, door mirror frames, spoilers, hood vents, spare tire covers, wheel covers, grille cover frames, light frames, door handles, door trims, rear surrounds, wipers, etc. In addition, the molded article of the present invention is also suitable as a sports product, and is suitable for golf clubs, clubs, grips, golf balls and other golf-related products, tennis rackets, tennis balls, badminton rackets, their strings and badminton shuttles and other racket sports-related products, American football, baseball, softball and other masks, helmets, chest protectors, elbow pads, knee pads and other sports body protection products, sports shoe bottom materials and other shoe-related products, fishing rods, reels, baits and other fishing gear-related products, surfing and other summer sports-related products, skiing, snowboards and other winter sports-related products, other indoor and outdoor sports-related products, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram showing a state in which organic fibers (A2) are enclosed in carbon fibers (A1) in a cross section of a molding material of a fiber-reinforced polyamide resin composition molded article.

[0039] Figure 2 This is a schematic diagram showing a state in which carbon fibers (A1) are enclosed by organic fibers (A2) in a cross section of a molding material of a fiber-reinforced polyamide resin composition molded article.

[0040] Figure 3 This is a schematic diagram showing a state in which a carbon fiber (A1) bundle and an organic fiber (A2) bundle exist separately in a state of being separated by a certain boundary portion in a cross section of a molding material of a fiber-reinforced polyamide resin composition molded article.

[0041] Figure 4 This is a schematic diagram of a composite fiber bundle (E) showing a state in which the component (D) adheres to a fiber bundle consisting of carbon fibers (A1) and organic fibers (A2) in a cross section of a molding material of a fiber-reinforced polyamide resin composition molded article. DETAILED DESCRIPTION

[0042] Hereinafter, the present invention will be described in detail together with embodiments.

[0043] The present invention is a fiber-reinforced polyamide resin composition molded article comprising a reinforcing fiber (A), a polyamide resin composition (B), and an ammonium salt (C) formed from an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia, wherein the reinforcing fiber (A) is 5 to 50 parts by weight, the polyamide resin composition (B) is 40 to 94.9 parts by weight, the aliphatic dicarboxylic acid having 6 to 12 carbon atoms and the ammonium salt (C) is 100 parts by weight of the total of the reinforcing fiber (A), the polyamide resin composition (B), and the ammonium salt (C) formed from an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia. The invention relates to a polyamide resin composition comprising: a polyamide resin (B1), a resin (B2) having a reactive functional group, and a compound (B3) formed by reacting (B1) with (B2), wherein the resin (B2) having a reactive functional group is dispersed in the form of particles having a number average particle size of 10 to 1,000 nm.

[0044] First, the fiber-reinforced polyamide resin composition molded article of the present invention is described in detail.

[0045] <Reinforcement fiber (A)>

[0046] The reinforcing fiber (A) in the present invention can improve the mechanical properties of the molded article by reinforcing the fiber of the polyamide resin composition (B). Furthermore, when the reinforcing fiber (A) has inherent properties such as electrical conductivity and thermal conductivity, those properties that cannot be obtained with the polyamide resin composition (B) alone can also be imparted to the molded article. In addition, for the purpose of imparting electrical conductivity, it is also preferred to use reinforcing fibers coated with metals such as nickel, copper, and ytterbium.

[0047] As reinforcing fiber, there is no particular limitation, and carbon fiber, organic fiber, glass fiber, metal fiber, etc. can be cited. Wherein, in order to improve mechanical properties, carbon fiber is more suitable for use. As carbon fiber, PAN (polyacrylonitrile) carbon fiber, asphalt carbon fiber, rayon carbon fiber, cellulose carbon fiber, vapor growth carbon fiber, their graphitized fibers, etc. can be exemplified. In the case of wanting to further improve impact properties, it is preferably used in combination with organic fiber described later.

[0048] As the carbon fiber, it is preferred that the surface oxygen concentration ratio [O / C] of the ratio of the number of atoms of oxygen (O) to carbon (C) on the fiber surface measured by X-ray photoelectron spectroscopy is 0.05 to 0.5. By having a surface oxygen concentration ratio of 0.05 or more, a sufficient amount of functional groups can be ensured on the surface of the carbon fiber, and a stronger adhesion with the polyamide resin composition (B) can be obtained, so that the bending strength and tensile strength of the molded product are further improved. The surface oxygen concentration ratio is more preferably 0.1 or more. In addition, from the perspective of the balance between the operability and productivity of the carbon fiber, the upper limit of the surface oxygen concentration ratio is more preferably 0.3 or less.

[0049] The surface oxygen concentration ratio of carbon fiber was obtained by X-ray photoelectron spectroscopy according to the following steps. First, if a sizing agent or the like was attached to the surface of the carbon fiber, the sizing agent or the like was removed with a solvent. The carbon fiber was cut into 20 mm pieces, spread and arranged on a copper sample support, and AlKα1,2 was used as an X-ray source. The sample chamber was kept at 1×10 -8 As a correction value for the charged peak accompanying the measurement, let C 1s The kinetic energy value (KE) of the main peak of C is consistent with 1202 eV. The C is obtained by drawing a straight line with a KE range of 1191 to 1205 eV as the baseline. 1s Peak area. The peak area was calculated by drawing a straight line with a baseline in the range of KE 947 to 959 eV. 1s Peak area.

[0050] Here, the surface oxygen concentration ratio [O / C] is given by the above O 1s Peak area and C 1sThe peak area ratio is calculated as the atomic ratio using the sensitivity correction value inherent in the device. As an X-ray photoelectron spectrometer, a model ES-200 manufactured by Kokusai Electric Co., Ltd. is used, and the sensitivity correction value is set to 1.74. The average fiber diameter of the carbon fiber is not particularly limited, but from the viewpoint of the mechanical properties and surface appearance of the molded product, it is preferably 1 to 20 μm, and more preferably 3 to 15 μm.

[0051] The carbon fibers may be surface treated for the purpose of improving the adhesion between the carbon fibers and the polyamide resin composition (B). Examples of the surface treatment method include electrolytic treatment, ozone treatment, and ultraviolet treatment.

[0052] The carbon fiber may be a carbon fiber to which a sizing agent is applied in order to prevent the fuzzing of the carbon fiber or to improve the adhesion between the carbon fiber and the polyamide resin composition (B). By applying a sizing agent, the surface characteristics such as the functional groups on the surface of the carbon fiber can be improved, and the adhesion and the mechanical properties (particularly impact strength) of the molded product can be improved.

[0053] As the sizing agent, for example, epoxy resin, phenol resin, polyethylene glycol, polyurethane, polyester, emulsifier or surfactant can be mentioned. Two or more of them can be used. The sizing agent is preferably water-soluble or water-dispersible. It is preferably an epoxy resin with excellent wettability with carbon fiber, and more preferably a multifunctional epoxy resin.

[0054] As the multifunctional epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, aliphatic epoxy resin, phenol novolac type epoxy resin, etc. can be cited. Among them, preferably an aliphatic epoxy resin that is easy to exert adhesion with the polyamide resin composition (B). Since the aliphatic epoxy resin is a soft skeleton, it is easy to form a structure with high toughness even if the cross-linking density is high. In addition, when the aliphatic epoxy resin is present between the carbon fiber / polyamide resin composition, it is soft and not easy to peel off, so the strength of the molded product can be further improved.

[0055] Examples of the multifunctional aliphatic epoxy resin include diglycidyl ether compounds, polyglycidyl ether compounds, etc. Examples of the diglycidyl ether compound include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ethers, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ethers, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, polybutylene glycol diglycidyl ethers, and polyalkylene glycol diglycidyl ethers. In addition, examples of the polyglycidyl ether compound include glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ethers, sorbitol polyglycidyl ethers, arabinitol polyglycidyl ethers, trimethylolpropane polyglycidyl ethers, trimethylolpropane glycidyl ethers, pentaerythritol polyglycidyl ethers, and polyglycidyl ethers of aliphatic polyhydric alcohols.

[0056] Among the above-mentioned aliphatic epoxy resins, trifunctional or higher aliphatic epoxy resins are preferred, and aliphatic polyglycidyl ether compounds having three or more highly reactive glycidyl groups are more preferred. The aliphatic polyglycidyl ether compounds have a good balance of flexibility, crosslinking density, and compatibility with the polyamide resin composition (B), and can further improve the adhesion. Among them, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ethers, polyethylene glycol glycidyl ethers, and polypropylene glycol glycidyl ethers are more preferred.

[0057] The amount of sizing agent attached is preferably 0.01 to 10 weight % in the total 100 weight % of sizing agent and carbon fiber. If the amount of sizing agent attached is 0.01 weight % or more, the adhesion to the polyamide resin composition (B) can be further improved. The amount of sizing agent attached is more preferably 0.05 weight % or more, and more preferably 0.1 weight % or more. On the other hand, if the amount of sizing agent attached is 10 weight % or less, the physical properties of the polyamide resin composition (B) can be maintained at a higher level. The amount of sizing agent attached is more preferably 5 weight % or less, and more preferably 2 weight % or less.

[0058] <Organic fiber (A2)>

[0059] For the fiber-reinforced polyamide resin composition molded product of the present invention, the above-mentioned reinforcing fiber (A) can contain the above-mentioned carbon fiber (A1) and organic fiber (A2). Carbon fiber (A1) is owing to being straight and brittle, and therefore is not easy to be wound and is easy to break. On the other hand, organic fiber (A2) is owing to having flexibility, and therefore is not easy to break during molding, and is easy to remain under the state of keeping long fiber length in the molded product. Therefore, by comprising soft and not easy to break organic fiber (A2), the impact characteristics of the molded product can be greatly improved.

[0060] Specifically, by setting the remaining fiber length of the organic fibers (A2) in the molded article (in other words, the weight average fiber length (Lwa2) in the molded article) to 3 mm or more and 7 mm or less, high impact properties can be imparted to the molded article.

[0061] Organic fiber (A2) can be appropriately selected within the range that the mechanical properties of the molded product are not greatly reduced. For example, polyester resins such as polyethylene, polypropylene, polyamide resins such as nylon 6, nylon 66, aromatic polyamide, polyethylene terephthalate, polybutylene terephthalate, polytetrafluoroethylene, perfluoroethylene / propylene copolymer, ethylene / tetrafluoroethylene copolymer, liquid crystal polyester, liquid crystal polymers such as liquid crystal polyester amide, polyether ketone, polyether sulfone, polyphenylene sulfide, etc., and the like can be cited. Fibers obtained by spinning resins such as polyarylether sulfides such as polyarylether sulfides. Two or more of them can be used. It is preferably appropriately selected from these organic fibers (A2) and used. In particular, it is preferred that the melting temperature of the organic fiber (A2) is 30°C to 150°C higher than the molding temperature (melting temperature) of the polyamide resin composition (B), and more preferably 50 to 100°C higher. Alternatively, the organic fiber (A2) made of a resin incompatible with the polyamide resin composition (B) is preferably used because it is directly present in the molded product while maintaining the fiber state, so the impact properties of the molded product can be further improved. As the organic fiber (A2) with a high melting temperature, polyphenylene sulfide resin, fluororesin, liquid crystal polyester fiber, etc. can be cited. As the organic fiber (A2) in the present invention, it is preferred to use at least one fiber selected from them.

[0062] The single fiber fineness of the organic fiber (A2) is preferably 0.1 to 50 dtex. It is more preferably 3 dtex or more, and further preferably 6 dtex or more. By making the single fiber fineness within the above range, the fiber shearing ability during molding is strong, so the fiber length in the molded product is easy to remain long, which can improve the impact strength of the molded product, and is therefore preferred.

[0063] The fiber strength of the organic fiber (A2) can be obtained by a known single-filament tensile test. Here, the fiber strength of the organic fiber (A2) can be calculated by conducting a tensile test in a room under standard conditions (20°C, 65% RH) at a clamp interval of 250 mm and a tensile speed of 300 mm / min, and dividing the load when the fiber is cut by the single-fiber fineness. Here, the so-called single-fiber fineness means the thickness of a yarn showing a weight of 1 g at a length of 10,000 m, and the single-fiber fineness of the organic fiber (A2) used in the present invention can be obtained by a known fiber fineness measurement (for example, JIS L 1013: 2010).

[0064] The fiber strength is preferably 4 cN / dtex or more. When it is less than 4 cN / dtex, the impact properties of the molded product are particularly reduced. It is more preferably more than 4 cN / dtex, further preferably more than 5 cN / dtex, and even more preferably more than 6 cN / dtex. In addition, the initial elastic modulus of the fiber can be calculated from the initial gradient in the stress-strain curve obtained with the above fiber strength.

[0065] The fiber strength is preferably 50 cN / dtex or less, more preferably 40 cN / dtex or less, and further preferably 30 cN / dtex or less. If the fiber strength exceeds 50 cN / dtex, it is not preferred because it becomes difficult to cut the fiber and the productivity of the molding material decreases.

[0066] The density of the organic fiber (A2) can be determined by a known density measurement (for example, JIS L 1015:2010).

[0067] The content of the organic fiber (A2) in the molded article of the present invention is preferably 1 to 50 parts by weight relative to 100 parts by weight of the total of the carbon fiber (A1) and the organic fiber (A2). When the content of the organic fiber (A2) is less than 1 part by weight, the impact properties of the molded article are reduced. The content of the organic fiber (A2) is more preferably 5 parts by weight or more, further preferably 10 parts by weight or more, and even more preferably 20 parts by weight or more. On the other hand, when the content of the organic fiber (A2) exceeds 50 parts by weight, the entanglement of the fibers often increases, the dispersibility of the organic fiber (A2) in the molded article is reduced, and the impact properties of the molded article are reduced. The content of the organic fiber (A2) is preferably 40 parts by weight or less, and more preferably 30 parts by weight or less. In addition, when the reinforcing fiber (A) of the fiber-reinforced polyamide resin composition molded article of the present invention contains carbon fiber (A1) and organic fiber (A2), the content of the carbon fiber (A1) is preferably 50 to 99 parts by weight relative to 100 parts by weight of the total of the carbon fiber (A1) and the organic fiber (A2). When the content of the carbon fiber (A1) is less than 50 parts by weight, it is difficult to obtain high mechanical properties of the molded article.

[0068] <Weight average fiber length>

[0069] For the fiber-reinforced polyamide resin composition molded product of the present invention, the weight-average fiber length (Lwa1) of the reinforcing fiber (A) in the molded product is 0.4 mm or more and 7.0 mm or less. When the weight-average fiber length (Lwa1) of the reinforcing fiber (A) is less than 0.4 mm, it is not easy to exert the flexural strength and impact characteristics of the molded product. Lwa1 is more preferably 0.5 mm or more, and more preferably 0.7 mm or more. On the other hand, when the weight-average fiber length (Lwa1) exceeds 7.0 mm, the entanglement between the monofilaments of the reinforcing fibers (A) is not easily suppressed, and fiber breakage occurs, so it is not easy to exert the flexural strength of the molded product. Lwa1 is more preferably 4 mm or less.

[0070] In addition, for the molded product of the present invention, when the reinforcing fiber (A) contains carbon fiber (A1) and organic fiber (A2), the weight average fiber length (Lwa2) of the organic fiber (A2) in the molded product is preferably 3 mm or more and 7 mm or less. When the weight average fiber length (Lwa2) of the organic fiber (A2) is less than 3 mm, the reinforcing effect of the organic fiber (A2) in the molded product is not easy to exert, and the impact characteristics are poor. Lwa2 is more preferably 4 mm or more. On the other hand, when the weight average fiber length (Lwa2) exceeds 7 mm, the entanglement between the monofilaments of the organic fiber (A2) is not easy to be suppressed, and fiber breakage occurs, so the impact characteristics of the molded product are poor. Lwa2 is more preferably 6 mm or less. By making the weight average fiber length (Lwa2) of the organic fiber (A2) the above range, the entanglement between the monofilaments of the organic fiber (A2) is suppressed, and the organic fiber (A2) exists in a bent state. As a result, the crack development when the molded product is destroyed becomes not in one direction, but can absorb more impact energy, so the impact strength of the molded product is improved.

[0071] Here, the so-called "weight average fiber length" in the present invention is not simply a number average, but refers to the average fiber length calculated by the following formula taking into account the contribution of fiber length by applying the calculation method of weight average molecular weight to the calculation of fiber length. The weight average fiber length of each of carbon fiber (A1) and organic fiber (A2) can be calculated by the following formula.

[0072] Weight average fiber length = Σ(Mi 2 ×Ni) / Σ(Mi×Ni)

[0073] Mi: Fiber length (mm)

[0074] Ni: The number of reinforcing fibers with a fiber length of Mi.

[0075] The weight average fiber length can be measured, for example, by heating a test piece of any size cut out from an ISO dumbbell test piece on a hot stage set at a temperature (e.g., 200 to 300° C.) at which the organic fiber (A2) does not melt but only the polyamide resin composition (B) melts, sandwiched between cover glasses, and forming a film without applying excessive pressure to uniformly disperse the test piece, thereby obtaining a film in which the fibers are uniformly dispersed; or by placing a test piece of any size cut out from an ISO dumbbell test piece into an organic solvent in which the organic fiber (A2) does not dissolve but only the polyamide resin composition (B) dissolves, heating and dissolving the test piece as needed, and filtering the organic solution to obtain an observation sample in which the fibers are uniformly dispersed. The sample obtained by the above method is observed with an optical microscope (50 to 200 times), and the fiber lengths of 1,000 randomly selected carbon fibers (A1) and organic fibers (A2) are measured, and the weight average fiber length (Lwa1) of the carbon fibers (A1) and the weight average fiber length (Lwa2) of the organic fibers (A2) are calculated from the above formula.

[0076] In addition, the weight average fiber length of the carbon fiber (A1) and the organic fiber (A2) in the molded product can be adjusted, for example, by molding conditions. As such molding conditions, for example, in the case of injection molding, pressure conditions such as back pressure and holding pressure, injection time, holding time and other time conditions, barrel temperature, mold temperature and other temperature conditions can be cited. Specifically, by utilizing that the organic fiber (A2) is softer and less prone to damage than the carbon fiber (A1), by appropriately increasing the pressure conditions such as back pressure, thereby appropriately increasing the shear force in the barrel, the average fiber length of the carbon fiber (A1) is shorter than that of the organic fiber (A2). In addition, by making the injection time appropriately short, the shear force during injection can be appropriately high, so that the average fiber length of the carbon fiber (A1) is shorter than that of the organic fiber (A2). If the temperature such as the barrel temperature and the mold temperature is further appropriately reduced, the viscosity of the flowing resin increases, and the shear force can be increased, so the average fiber length of the carbon fiber (A1) can also be made shorter than that of the organic fiber (A2) by such a method. In the present invention, by appropriately changing the conditions as described above, the average fiber length of the carbon fiber (A1) and the organic fiber (A2) in the molded product can be within the desired range. Among them, it is particularly effective to adjust the shear force by controlling the back pressure conditions and injection time. However, if the shear force acting on the fiber is excessively increased to a level higher than necessary, the average fiber length of not only the carbon fiber (A1) but also the organic fiber (A2) will be shortened, so it is necessary to pay attention.

[0077] <Polyamide resin composition (B)>

[0078] The polyamide resin composition used in the present invention comprises a polyamide resin (B1), a resin having a reactive functional group (B2), and a compound (B3) produced by the reaction of (B1) and (B2).

[0079] <Polyamide resin (B1)>

[0080] The polyamide resin (B1) is a resin composed of a polymer having an amide bond, and uses amino acids, lactams or diamines and dicarboxylic acids as main raw materials. Representative examples of such raw materials include amino acids such as (6-aminocaproic acid), (11-aminoundecanoic acid), (12-aminododecanoic acid), and p-aminomethylbenzoic acid; lactams such as ε-caprolactam and ω-laurolactam; 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 2-methyl1,5-pentanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 2,2,4- / 2,4,4-trimethyl1,6-hexanediamine, 5-methyl1,9-nonanediamine, m-xylylenediamine, p-xylylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane , 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, aminoethylpiperazine and other aliphatic, alicyclic or aromatic diamines; and adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid and other aliphatic, alicyclic or aromatic dicarboxylic acids. In the present invention, the polyamide homopolymers or copolymers derived from these raw materials can be used alone or in the form of a mixture.

[0081] In the present invention, specific examples of particularly useful polyamides include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polypentamethylene adipamide (nylon 56), polybutylene adipamide (nylon 46), polyhexamethylene sebacamide (nylon 610), polypentamethylene sebacamide (nylon 510), polyhexamethylene dodecanamide (nylon 612), polyundecanamide (nylon 11), polydodecanamide (nylon 12), polycaproamide / polyhexamethylene adipamide copolymer (nylon 6 / 66), polycaproamide / polyhexamethylene terephthalamide copolymer (nylon 6 / 6T), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6T), polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6 I), polyhexamethylene adipamide / polyhexamethylene isophthalamide / polycaproamide copolymer (nylon 66 / 6I / 6), polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 6T / 6I), polyhexamethylene terephthalamide / polydodecanoamide copolymer (nylon 6T / 12), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyphenylene adipamide (nylon XD6), polyhexamethylene terephthalamide / poly-2-methylpentamethylene terephthalamide copolymer (nylon 6T / M5T), polyhexamethylene terephthalamide / polypentamethylene terephthalamide copolymer (nylon 6T / 5T), polynonane terephthalamide (nylon 9T) and mixtures or copolymers thereof, etc.

[0082] As particularly preferred materials, nylon 6, nylon 66, nylon 610, nylon 11, nylon 12, nylon 6 / 66, nylon 66 / 6T, nylon 6T / 6I copolymers and the like can be cited. Furthermore, it is also practically suitable to use these polyamides as a mixture according to the required properties such as moldability, heat resistance, toughness, and surface properties. Among them, nylon 6, nylon 66, nylon 610, nylon 11, and nylon 12 are most preferred.

[0083] In addition, the molded article of the present invention preferably comprises a mixture of a polyamide resin (B1a) comprising polyamide 6 or polyamide 66 as a constituent component and one or more polyamide resins (B1b) selected from polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 1012, polyamide 9T, and a copolymer polyamide comprising at least one of these as a constituent component. The polyamides are characterized by being a mixture based on the necessary properties such as moldability, heat resistance, toughness, and surface properties. The polyamide resin (B1b) is a polyamide resin having a water absorption of 5% or less when placed in a 25°C water environment for 300 hours. By appropriately adjusting the mixing ratio of the polyamide resins (B1a) and (B1b), the water absorption of the molded article when placed in an 80°C × 95% RH environment for 24 hours can be suppressed to 3.0% or less, thereby suppressing the reduction in rigidity of the molded article when it absorbs water. If the water absorption rate exceeds 3.0%, the rigidity decreases significantly when absorbing water, which is not preferred. The water absorption rate is more preferably 2.7% or less.

[0084] In addition, in the present invention, it is clarified that the fiber dispersibility is improved by selecting a material having an SP value between (B1a) and the resin (B2) described later, with respect to the polyamide resin (B1b). Although the mechanism is presumed, it is considered that the SP value of the polyamide 6 resin (B1a) and the resin (B2) described later is controlled by (B1b) by mixing the polyamide resin (B1b). That is, it is presumed that the compatibility with the carbon fiber (A1) and the organic fiber (A2) is further improved by (B1b) being located between (B1a) and (B2) whose SP values ​​are far apart.

[0085] From the viewpoint of water absorption and fiber dispersibility, it is preferred that polyamide 6 resin be selected as (B1a) and polyamide 610 be selected as (B1b) among these combinations.

[0086] The polymerization degree of these polyamides is not particularly limited, but the relative viscosity measured at 25°C in a 98% concentrated sulfuric acid solution having a sample concentration of 0.01 g / ml is preferably in the range of 1.5 to 7.0, and particularly preferably in the range of 1.8 to 5.0. If the relative viscosity is 1.5 or more, high impact resistance is imparted by the fiber-reinforced resin composition. In addition, if the relative viscosity is 7.0 or less, excellent moldability is achieved.

[0087] <Resin having a reactive functional group (B2)>

[0088] The resin used as the base of the resin (B2) having a reactive functional group is not particularly limited, and can be selected from, for example, polyamide, polyester, polyphenylene sulfide, polyphenylene ether, polycarbonate, polylactic acid, polyacetal, polysulfone, tetrafluoroethylene, polyetherimide, polyamideimide, polyimide, polyethersulfone, polyetherketone, polythioetherketone, polyetheretherketone, polyethylene, polypropylene, polystyrene, styrene resins such as ABS, rubber polymers, polyoxyalkylenes, etc., and at least one resin different from the above-mentioned polyamide resin (B1) can be used. Among them, the resin used as the base of the resin (B2) is more preferably a resin selected from polyolefin resins such as polyethylene resins and polypropylene resins, styrene resins, and rubber polymers from the viewpoint of easy introduction of reactive functional groups, and is more preferably a rubber polymer from the viewpoint of imparting impact absorption.

[0089] The rubber polymer is a polymer having a low glass transition temperature, in which a part of the molecules are bound by covalent bonds, ionic bonds, van der Waals forces, entanglement, etc. The glass transition temperature of the rubber polymer is preferably 25° C. or less. If the glass transition temperature exceeds 25° C., the impact resistance is poor, which is not preferred.

[0090] Examples of the rubber polymer include polybutadiene, polyisoprene, random copolymers and block copolymers of styrene-butadiene, hydrogenated products of the block copolymers, diene rubbers such as acrylonitrile-butadiene copolymers and butadiene-isoprene copolymers, random copolymers and block copolymers of ethylene-propylene, random copolymers and block copolymers of ethylene-butene, copolymers of ethylene and α-olefins, ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers, ethylene-unsaturated carboxylic acid ester copolymers such as ethylene-acrylate and ethylene-methacrylate, and unsaturated carboxylic acid ester copolymers in which a part of the unsaturated carboxylic acid is Preferred examples include metal salts of ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid metal salt copolymers such as ethylene-acrylic acid-acrylic acid metal salt, ethylene-methacrylic acid-methacrylic acid metal salt, acrylic ester-butadiene copolymers such as butyl acrylate-butadiene copolymer, copolymers of ethylene and fatty acid vinyl esters such as ethylene-vinyl acetate, ethylene-propylene-ethylidene norbornene copolymers, ethylene-propylene non-conjugated diene terpolymers such as ethylene-propylene-hexadiene copolymer, butene-isoprene copolymers, chlorinated polyethylene, polyamide elastomers, polyester elastomers and other thermoplastic elastomers.

[0091] When the polyamide resin (B1) is used, it is preferred to use ethylene-unsaturated carboxylic acid ester copolymers, random copolymers and block copolymers of ethylene-propylene, random copolymers and block copolymers of ethylene-butene, and copolymers of ethylene and α-olefins from the viewpoint of obtaining excellent impact strength.

[0092] As the unsaturated carboxylic acid ester in the ethylene-unsaturated carboxylic acid ester copolymer, (meth)acrylate is preferred. Specific examples of unsaturated carboxylic acid esters include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate. Here, "(meth)acrylic acid" refers to "acrylic acid or methacrylic acid". The weight ratio of the ethylene component to the unsaturated carboxylic acid ester component in the copolymer is not particularly limited, but is preferably in the range of 90 / 10 to 10 / 90, and more preferably in the range of 85 / 15 to 15 / 85. The number average molecular weight of the ethylene-unsaturated carboxylic acid ester copolymer is not particularly limited, but from the viewpoint of fluidity and mechanical properties, it is preferably in the range of 1,000 to 70,000.

[0093] The reactive functional group contained in the resin (B2) having a reactive functional group is not particularly limited as long as it reacts with the functional group present in the polyamide resin (B1), but preferably includes an amino group, a carboxyl group, a metal salt of a carboxyl group, a hydroxyl group, an epoxy group, an acid anhydride group, an isocyanate group, a mercapto group, At least one selected from amino, carboxyl, metal salt of carboxyl, epoxy, anhydride and The group in the oxazoline group is more preferably used because it has high reactivity and less side reactions such as decomposition and cross-linking.

[0094] When introducing an acid anhydride group into a rubber polymer, the method can be carried out by a known technique without particular limitation. For example, a method of copolymerizing an acid anhydride such as maleic anhydride, itaconic anhydride, nadic anhydride, citraconic anhydride, 1-butene-3,4-dicarboxylic anhydride and a monomer as a raw material of the rubber polymer, a method of grafting an acid anhydride onto the rubber polymer, etc. can be used.

[0095] When introducing an epoxy group into a rubber polymer, the method can be carried out by a known technique without particular limitation. For example, a method of copolymerizing a vinyl monomer having an epoxy group such as a glycidyl ester compound of an α,β-unsaturated acid such as glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, or glycidyl itaconate with a monomer as a raw material of the rubber polymer; a method of polymerizing a rubber polymer using a polymerization initiator or chain transfer agent having an epoxy group; a method of grafting an epoxy compound onto a rubber polymer, and the like can be used.

[0096] In addition, When an oxazoline group is introduced into a rubber polymer, the method can be carried out by a known technique without particular limitation. For example, 2-isopropenyl- Oxazoline, 2-vinyl- Oxazoline, 2-acryloyl- Oxazoline, 2-phenylvinyl- Oxazoline and others have A method of copolymerizing an oxazoline-based vinyl monomer with a monomer serving as a raw material for a rubbery polymer.

[0097] The number of functional groups per molecular chain in the resin (B2) having a reactive functional group is not particularly limited, but is usually preferably 1 to 10, and preferably 1 to 5 in order to reduce side reactions such as crosslinking.

[0098] The polyamide resin composition (B) of the present invention is composed of a polyamide resin (B1), a resin (B2) having a reactive functional group, and a compound (B3) generated by the reaction of (B1) and (B2). The above-mentioned polyamide resin composition (B) can be obtained by melt-kneading the polyamide resin (B1) and (B2) having a reactive functional group. In addition, since (B2) has a reactive functional group, (B3) is generated by the reaction of (B1) and (B2) during the melt-kneading of (B1) and (B2). A polyamide resin composition (B) in which (B1) forms a matrix phase as a continuous layer and (B2) is dispersed in a particle form as a dispersed phase can be obtained. The structure of the particles formed by (B2) is highly controlled, which greatly contributes to the improvement of impact resistance. The polyamide resin (B1) and the component (B) are mixed to form a matrix resin, and the number average particle size of the particles formed by the resin (B2) contained in the polyamide resin composition (B) in which the resin (B2) is dispersed in the form of particles of the matrix resin needs to be 10 to 1,000 nm. If the number average particle size of the particles is less than 10 nm, the impact resistance that is a feature of the present invention cannot be exhibited, and if it exceeds 1,000 nm, the rigidity that is a feature of the present invention is reduced, which is not desirable. By achieving improved impact resistance with a small amount of particles formed by the resin (B2) with a highly controlled structure, a fiber-reinforced polyamide resin composition molded product with an excellent balance between rigidity and impact resistance can be obtained.

[0099] Furthermore, the fiber-reinforced polyamide resin composition molded article of the present invention preferably contains a compound (B3) having an average particle size of 1 to 100 nm generated by the reaction of a polyamide resin (B1) and a resin (B2) in the particles formed by the resin (B2). It is further preferred that the area ratio occupied by the compound (B3) generated by the reaction of the above-mentioned components (B1) and (B2) in the particles formed by the resin (B2) is 20% or more. Even if the blending amount of the resin (B2) forming the dispersed phase is small, a fiber-reinforced polyamide resin composition molded article having an excellent balance between rigidity and impact resistance can be obtained by controlling the structure in the dispersed phase as described above.

[0100] In addition, the morphological observation method can apply known techniques. For example, the central part of the cross-sectional direction of the test piece is cut into 1-2 mm squares, and the resin (B2) having a reactive functional group is dyed with ruthenium tetroxide, and then an ultrathin slice with a thickness of less than 0.1 μm (about 80 nm) is obtained by an ultrathin slicer, and the resin part (excluding the part of the reinforcing fiber) composed of the polyamide resin (B1), the resin (B2) and the compound (B3) of the slice is observed with a transmission electron microscope. With regard to the number average particle size (Xn) of the particles, more than 400 particles are randomly selected from the obtained image, and the particle size distribution is analyzed using the image analysis software "Scion Image" made by Scion Corporation, and the following formula is used to obtain it.

[0101] Number average particle size (Xn) = Σ(Xi×ni) / Σni

[0102] Xi; particle size

[0103] ni; number of particles that match the particle size (Xi)

[0104] (i=1、2、3、···、n)

[0105] The number average particle size of the particles formed by the resin (B2) can be obtained from an image magnified 10,000 times. In addition, the number average particle size of the compound (B3) generated by the reaction of the polyamide resin (B1) and (B2) contained in the particles formed by (B2) can be obtained from an image magnified 35,000 times.

[0106] The area ratio of the compound (B3) in the particles formed by the resin (B2) was obtained by analyzing the area of ​​the resin (B2) and the area occupied by the compound (B3) separately using the image analysis software "Scion Image" manufactured by Scion Corporation using a transmission electron microscope and the image was magnified 35,000 times, and the result was calculated using the following formula.

[0107] Sn=Sp / (Sa2+Sp)

[0108] Sn; Area ratio (Sn) of the compound (B3) in the particles formed of the resin (B2)

[0109] Sa2: Area occupied by resin (B2)

[0110] Sp; area occupied by compound (B3).

[0111] In the present invention, the method for producing the polyamide resin composition (B) is not particularly limited, and for example, the following method is effective.

[0112] As one of the methods for producing the polyamide resin composition (B), there is mentioned a method of introducing a polyamide resin (B1) and a resin (B2) having a reactive functional group into a twin-screw extruder having a ratio L / D0 of screw length L to screw diameter D0 of 50 or more and having a plurality of full-flight regions and kneading regions, and melt-kneading the mixture under the condition that Pkmax ≥ Pfmin + 0.3, when the maximum resin pressure among the resin pressures in the kneading regions of the screw is set to Pkmax (MPa) and the minimum resin pressure among the resin pressures in the full-flight regions of the screw is set to Pfmin (MPa).

[0113] From the perspective of improved kneading properties and reactivity, the value of L / D0 is more preferably 60 to 200, and is further preferred if it is in the range of 80 to 200. In addition, when using a twin-screw extruder with an L / D0 of less than 50, the calculated L / D0 value through which the resin composition passes is preferably 50 or more by performing multiple kneading. L / D0 is the value obtained by dividing the screw length L by the screw diameter D0. Here, the so-called screw length is the length from the end of the upstream side of the screw segment of the position (feed port) where the polyamide resin (B1) and the resin (B2) having a reactive functional group are supplied to the root of the screw to the front end of the screw. The screw of the twin-screw extruder is composed of screw segments with different characteristics such as full flight and kneading disk in length and shape. In addition, in the extruder, the side that supplies the raw materials is sometimes called the upstream, and the side that discharges the molten resin is sometimes called the downstream.

[0114] When a twin-screw extruder having an L / D0 of 50 or more is used to produce the polyamide resin composition (B), it is preferred that the screw of the twin-screw extruder has a plurality of full-flight regions and kneading regions from the perspective of improved kneading properties and reactivity. The full-flight region is composed of one or more full-flights, and the kneading region is composed of one or more kneading disks.

[0115] If the resin pressure of the kneading area which is the largest among the resin pressures displayed by the resin pressure gauges at multiple locations in the kneading area is set to Pkmax (MPa), and the resin pressure of the full thread area which is the smallest among the resin pressures displayed by the resin pressure gauges at multiple locations in the full thread area is set to Pfmin (MPa), it is preferred to manufacture under the condition that the Pkmax value is greater than (Pfmin+0.3), and it is more preferred to manufacture under the condition that the Pkmax value is greater than (Pfmin+0.5).

[0116] The kneading area composed of more than one kneading disk is superior to the full-thread area composed of more than one full-thread. The kneading and reactivity of the molten resin are improved by filling the kneading area with molten resin. As an indicator showing the full state of the molten resin, there is a value of resin pressure, and the greater the resin pressure, the more the molten resin is filled. That is, when using a twin-screw extruder, the reaction can be effectively promoted by increasing the resin pressure in the kneading area within a certain range compared to the resin pressure in the full-thread area.

[0117] There are no particular limitations on the method for increasing the resin pressure in the kneading zone, but preferably, a method of introducing a reverse screw zone having an effect of pushing the molten resin back to the upstream side, a seal ring zone having an effect of storing the molten resin, etc., between the kneading zones or on the downstream side of the kneading zone can be used. The reverse screw zone and the seal ring zone are composed of one or more reverse screws and one or more seal rings, and these can also be combined.

[0118] For example, when an anti-screw zone is introduced between kneading zones or on the downstream side of the kneading zone, if the length of the anti-screw zone is set to Lr, it is preferred that the anti-screw zone has a length of Lr / D0=0.1 to 10 from the viewpoint of kneading property and reactivity. The length Lr / D0 of the anti-screw zone is more preferably 0.2 to 8, and further preferably 0.3 to 6. When a plurality of anti-screw zones are provided, it is preferred that all anti-screw zones satisfy the above-mentioned range of Lr / D0. In addition, the length Lr of the anti-screw zone is set to be the distance between the perpendicular line from the upstream end of the most upstream anti-screw constituting the anti-screw zone to the center line of the screw shaft, and the perpendicular line from the downstream end of the most downstream anti-screw constituting the anti-screw zone to the center line of the screw shaft.

[0119] When a twin-screw extruder having an L / D0 of 50 or more is used to produce the polyamide resin composition (B), the extrusion rate is preferably 0.01 kg / h or more, more preferably 0.05 kg / h to 1 kg / h, further preferably 0.08 to 0.5 kg / h, and most preferably 0.1 to 0.3 kg / h per 1 rpm of the screw. The extrusion rate here refers to the weight (kg) of the molten kneaded material discharged from the extruder per hour.

[0120] In addition, the preferred numerical range related to the extrusion amount in the above-mentioned twin screw extruder is based on the extrusion amount of a twin screw extruder with a screw diameter of 41 mm. In other words, when the screw diameter is greatly different, for example, when a twin screw extruder with a diameter of less than 30 mm or a diameter of more than 50 mm is used, the extrusion amount can be a value that is reduced or increased, preferably by 2.5 or 3, more preferably by 2.5, relative to the ratio of the screw diameter before and after proportional reduction or proportional expansion.

[0121] For example, when using a twin-screw extruder with a screw diameter of 20 mm, if the extrusion amount is 2.5 times the ratio of the screw diameters before and after proportional reduction, the extrusion amount of the molten kneaded product is per 1 rpm of screw speed, preferably 0.0017 kg / h or more, more preferably 0.0083 to 0.17 kg / h, further preferably 0.013 to 0.083 kg / h, and most preferably 0.017 to 0.050 kg / h.

[0122] In addition, when using a twin-screw extruder with a screw diameter of 100 mm, if the extrusion amount is proportionally enlarged according to the 2.5th power of the screw diameter ratio before and after, the extrusion amount of the molten kneaded product is per 1 rpm of the screw, preferably 0.093 kg / h or more, more preferably 0.46 to 9.29 kg / h, further preferably 0.74 to 4.65 kg / h, and most preferably 0.93 to 2.79 kg / h.

[0123] The rotation speed of the screw is not particularly limited, but is preferably 10 rpm or more, more preferably 15 rpm or more, and even more preferably 20 rpm or more.

[0124] The residence time in the twin-screw extruder is preferably 1 to 30 minutes, more preferably 1.5 to 25 minutes. Such so-called residence time is an average value representing the residence time from the supply of raw materials to the twin-screw extruder to the discharge. The residence time is set to be the time when the colorant is put into the position of the screw root where the raw material is supplied together with the raw material under the stable melt-kneading state where the non-colored molten kneaded material is adjusted to a specified extrusion amount, and the colorant is put into the extruded material together with the raw material, from the time when the colorant is put into the extruded material from the discharge port of the extruder and the coloring degree caused by the colorant to the extruded material becomes the maximum.

[0125] When a twin-screw extruder with L / D0 of more than 50 is used to manufacture the polyamide resin composition (B), there is no particular limitation on the screw of the twin-screw extruder, and screws of a completely intermeshing type, an incompletely intermeshing type, a non-intermeshing type, etc. can be used. From the viewpoint of kneadability and reactivity, a completely intermeshing type screw is preferably used. In addition, as the direction of rotation of the screw, the same direction or different directions are all acceptable, but from the viewpoint of kneadability and reactivity, it is preferably rotated in the same direction. As the screw, the most preferred is a completely intermeshing type that rotates in the same direction.

[0126] As the screw structure of the twin-screw extruder, although a combination of full flight and / or kneading disks is used, it is preferred that the screw structure effectively imparts a shear field to the resin composition in a molten state. Therefore, as described above, it is preferred that the screw of the twin-screw extruder has kneading areas composed of one or more kneading disks at multiple locations along the length direction. The total length of these kneading areas is preferably 5 to 50% of the total length of the screw, more preferably 10 to 40%, and further preferably in the range of 15 to 30%.

[0127] From the viewpoint of kneading property and reactivity, if the length of each kneading zone in the screw of the twin-screw extruder is set to Lk, it is preferred that all kneading zones have a length of Lk / D0=0.2 to 10. The length Lk / D0 of each kneading zone is more preferably 0.3 to 9, and further preferably 0.5 to 8. In addition, the length Lk of the kneading zone is set to the distance between the perpendicular line from the upstream end of the most upstream kneading disk constituting the kneading zone to the center line of the screw shaft, and the perpendicular line from the downstream end of the most downstream kneading disk constituting the kneading zone to the center line of the screw shaft. In addition, the kneading zone of the twin-screw extruder is preferably not offset at a specific position in the screw, but is configured throughout the entire area.

[0128] In order to remove reaction by-products or thermally degraded substances, etc., it is preferred to set a vented vacuum area and reduce the pressure to a pressure below -0.07 MPa, and more preferably to reduce the pressure to a pressure below -0.08 MPa. The so-called gauge pressure here means the pressure when the atmospheric pressure is set to zero. The lower the pressure, the higher the vacuum degree and the higher the ability to remove volatile components. When the gauge pressure in the vented vacuum area exceeds -0.07 MPa, that is, when the vacuum degree is low, the above-mentioned volatile components cannot be fully removed, and impurities remain in the polyamide resin composition (B), so it is not preferred. By fully removing the volatile components in the vented vacuum area, the amount of impurities in the melt-kneaded product can be reduced. There is no particular restriction on the number of vented vacuum areas, and it is preferably set to 1 to 10. In addition, there is no particular restriction on the position of the vented vacuum area, but it is preferred to set at least one position closer to the sampling position at L / D0=0 to 10 to effectively remove the above-mentioned volatile components.

[0129] It is preferred that the maximum resin temperature be controlled to be 180°C to 330°C for melt kneading, and more preferably 200°C to 325°C for melt kneading. The maximum resin temperature here refers to the highest temperature during measurement using resin thermometers evenly set at multiple positions of the extruder. When the maximum resin temperature is less than 180°C, the reactivity between polymers is low, and when it exceeds 330°C, thermal decomposition of the polymer proceeds.

[0130] When a twin-screw extruder is used, in order to suppress thermal degradation, it is preferred to introduce an inert gas from the raw material input portion for melt kneading. The inert gas is preferably nitrogen.

[0131] As a second method for producing the polyamide resin composition (B), there can be mentioned a method of melt-kneading the polyamide resin (B1) and the resin (B2) having a reactive functional group by extensional flow. Compared with the shear flow generally used in melt-kneading, the extensional flow kneading has a high dispersion efficiency, so the reaction is efficiently carried out, especially in the case of alloying accompanied by reaction such as reactive processing.

[0132] When the polyamide resin composition (B) is manufactured by melt-mixing while stretching the flow, it is preferred to utilize melt-mixing using an extruder. As examples of extruders, single-screw extruders, twin-screw extruders, and multi-screw extruders with more than three screws can be cited. Among them, single-screw extruders and twin-screw extruders are preferably used, and twin-screw extruders are particularly preferably used. In addition, as the screw of such a twin-screw extruder, there is no particular restriction, and screws of a completely intermeshing type, an incompletely intermeshing type, a non-intermeshing type, etc. can be used. From the viewpoint of compatibility and reactivity, it is preferably a completely intermeshing type. In addition, as the direction of rotation of the screw, the same direction and different directions are all OK, but from the viewpoint of compatibility and reactivity, it is preferably rotated in the same direction. The most preferred screw is a completely intermeshing type that rotates in the same direction.

[0133] In order to provide an elongational flow field suitable for reactive processing, the ratio of the total length of the elongational flow regions to the total length of the extruder screw is preferably in the range of 5 to 60%, more preferably 10 to 55%, and even more preferably 15 to 50%.

[0134] If the length of the extensional flow zone in the screw of the extruder is set to Lk and the screw diameter is set to D0, then from the viewpoint of kneading property and reactivity, Lk / D0 is preferably 0.2 to 10. More preferably, it is 0.3 to 9, and further preferably 0.5 to 8. In the case where multiple extensional flow zones are provided, it is preferred that all of the extensional flow zones satisfy the above-mentioned range of Lk / D0. In addition, in the present invention, the extensional flow zone is preferably not biased to a specific position in the screw, but is configured throughout the entire area.

[0135] As the screw structure of the extensional flow region, there can be cited: a torsion kneading disk composed of a kneading disk, in which the helical angle θ between the top of the front end side of the disk and the top of the rear end side thereof is in the range of 0°<θ<90° along the half-rotation direction of the screw; a screw composed of a threaded screw, in which a resin passage whose cross-sectional area is reduced from the front end side of the screw toward the rear end side is formed in the threaded portion of the screw; and a resin passage whose cross-sectional area is temporarily reduced to allow molten resin to pass through in an extruder as preferred examples.

[0136] Preferably, the extrusion rate relative to the screw 1rpm is more than 0.01kg / h. The so-called extrusion rate is the weight (kg) of the molten kneaded material discharged from the extruder per hour. If the extrusion rate relative to the screw 1rpm is less than 0.01kg / h, the extrusion rate relative to the rotation speed is insufficient, the residence time in the extruder is too long, which becomes the cause of thermal degradation, and the filling rate of the resin in the extruder becomes very small, and it is not possible to fully mix such a problem. In addition, as the rotation speed of the screw, there is no particular restriction, but it is preferably more than 10rpm, more preferably more than 50rpm, and more preferably more than 80rpm. In addition, the extrusion rate is preferably more than 0.1kg / h, more preferably more than 0.15kg / h, and more preferably more than 0.2kg / h.

[0137] The residence time in the extruder is preferably 1 to 30 minutes, more preferably 1.5 to 28 minutes, and further preferably 2 to 25 minutes. The so-called residence time is an average value representing the residence time from supplying raw materials to discharge to the extruder. The residence time is set to be a stable melt-kneading state in which the uncolored resin composition is adjusted to a specified extrusion amount, and about 1g of colorant is added together with the raw materials from the position of the screw root of the raw material supply, from the moment of adding the colorant, etc. to the moment when the coloring degree caused by the colorant to the extrudate becomes the maximum from the discharge port of the extruder. When the residence time is less than 1 minute, the reaction time in the extruder is short, and the reaction will not be fully promoted, so it is not preferred. When the residence time is longer than 30 minutes, thermal degradation of the resin caused by the long residence time occurs, so it is not preferred.

[0138] When a polyamide resin composition (B) is manufactured using a twin-screw extruder with an L / D0 of 50 or more, or when a polyamide resin composition (B) is manufactured by melt kneading simultaneously with extensional flow, if the mixing ratio of the polyamide resin (B1) and the resin (B2) having a reactive functional group is 80 to 60% by weight of the polyamide resin (B1) and 20 to 40% by weight of the resin (B2), the polyamide resin (B1) forms a continuous phase, the resin (B2) forms a dispersed phase, and the particles formed by the resin (B2) contain a compound (B3) of 1 to 100 nm generated by the reaction of (B1) and (B2), and the area ratio occupied by the compound (B3) tends to be 20% or more, which is preferred.

[0139] <Ammonium salt (C)>

[0140] The polyamide resin composition of the present invention contains an ammonium salt (ammonium salt (C)) formed from an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia. For the sake of caution, the ammonium salt (C) is (R(COO - )2·(NH4 + The compound represented by the chemical formula of )2) (here, R is a divalent aliphatic group having 4 to 10 carbon atoms), in which the hydrogen atom of the ammonium ion is replaced by one or more functional groups other than hydrogen atoms, and the primary ammonium salt, secondary ammonium salt, tertiary ammonium salt, and quaternary ammonium salt do not meet the so-called ammonium salt (C) in the present invention.

[0141] It is presumed that when an aliphatic dicarboxylic acid having 6 to 12 carbon atoms is used instead of the ammonium salt (C), such an aliphatic dicarboxylic acid has a high affinity with the polyamide resin (B1) contained in the polyamide resin composition (B), as when it is used as a raw material of the polyamide resin composition (B). In addition, the amino group of the polyamide resin (B1) contained in the polyamide resin composition (B) can react with the carboxyl group of the aliphatic dicarboxylic acid, so the aliphatic dicarboxylic acid is dispersed to a certain extent in the polyamide resin (B1) contained in the polyamide resin composition (B). However, since the aliphatic dicarboxylic acid is an acid, if the content increases, the polyamide resin (B1) contained in the polyamide resin composition (B) is decomposed, and the mechanical properties of the obtained molded article are reduced.

[0142] On the other hand, it is presumed that the ammonium salt of an aliphatic dicarboxylic acid having 5 or less carbon atoms has a high affinity with the polyamide resin (B1) contained in the polyamide resin composition (B), and therefore is dispersed in the polyamide resin (B1) contained in the polyamide resin composition (B). However, since the ammonium salt of an aliphatic dicarboxylic acid having 5 or less carbon atoms has a low molecular weight, the ammonium salt is decomposed during the production of the polyamide resin (B1) contained in the polyamide resin composition (B), and thus the mechanical properties of the obtained molded article are reduced.

[0143] When the ammonium salt (C) formed of an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia proposed in the present invention is used, the following actions and effects can be obtained.

[0144] That is, since it can be considered that the ammonium salt (C) is coordinated with the amide group or carboxyl terminal group of the polyamide resin (B1) contained in the polyamide resin composition (B), the ammonium salt (C) has excellent compatibility with the polyamide resin (B1) contained in the polyamide resin composition (B), can be micro-dispersed in the polyamide resin composition, and improves the fluidity of the polyamide resin composition (B). Further, since the ammonium salt (C) with modified fluidity shows good affinity to the polyamide resin (B1) contained in the polyamide resin composition (B), the fiber dispersibility of the reinforcing fiber (A) in the case of forming a fiber-reinforced polyamide resin molded product is not damaged, so the reinforcing fiber (A) can be dispersed as a single filament inside the molded product, and the fiber dispersibility of the molded product can be improved. In addition, the ammonium salt (C) shows high affinity to the polyamide resin (B1), so it is also excellent in suppressing the oozing to the surface of the molded product.

[0145] In addition, since the ammonium salt (C) has a higher molecular weight than the ammonium salt formed by an aliphatic dicarboxylic acid having a carbon number of 5 or less and ammonia, the decomposition / volatilization of the ammonium salt (C) is suppressed. In addition, since the ammonium salt (C) is neutral, even if it is contained in a large amount, the decomposition of the polyamide resin caused by acid or alkali during the manufacture of the polyamide composition is suppressed. Therefore, the fluidity of the polyamide resin composition (B) can be more effectively improved, and the mechanical properties and appearance quality of the obtained molded article can be improved.

[0146] Specific examples of the ammonium salt (C) include diammonium adipate, diammonium pimelate, diammonium suberate, diammonium azelate, diammonium sebate, ammonium dodecanedioate, etc. Two or more kinds may be used as required. Among them, diammonium adipate and diammonium sebate are preferably used from the viewpoint of raw material availability, performance balance, and cost.

[0147] In the fiber-reinforced polyamide resin composition molded article of the present invention, the content of the ammonium salt (C) is 0.1 to 10 parts by weight relative to 100 parts by weight of the total of the reinforcing fiber (A), the polyamide resin composition (B) and the ammonium salt (C). If the content of the ammonium salt (C) is less than 0.1 parts by weight, the fluidity, fiber dispersibility and mechanical properties of the fiber-reinforced polyamide resin composition (B) are reduced. The content of the ammonium salt (C) is preferably 0.2 parts by weight or more, and more preferably 0.3 parts by weight or more, relative to 100 parts by weight of the total of the reinforcing fiber (A), the polyamide resin composition (B) and the ammonium salt (C). On the other hand, if the content of the ammonium salt (C) exceeds 10 parts by weight, the plasticization of the polyamide resin (B1) is promoted, and the mechanical properties of the resulting molded article are reduced. The content of the ammonium salt (C) is preferably 5 parts by weight or less, more preferably 3 parts by weight or less, and more preferably 1.5 parts by weight or less, relative to 100 parts by weight of the total of the reinforcing fiber (A), the polyamide resin composition (B) and the ammonium salt (C).

[0148] In addition, the content of the ammonium salt (C) and the content of the ammonium ion [B] in the resin composition were determined by the following method.

[0149] In the case of incompatible components such as inorganic particles and organic particles included in the polyamide resin composition, these components are directly or converted into other forms such as oxides and separated, and the amount contained by the per unit weight of the polyamide resin composition is obtained. As the method of separation, it is possible to appropriately select according to the component included, without particular restriction. On the other hand, in the case of other organic components or inorganic components including compatibility, the component that can be separated by extraction of water, organic solvents etc. is separated by extraction and the amount contained by the per unit weight of the polyamide resin composition is obtained, and in the case of its difficulty, the containing rate in the composition is obtained according to the analytical methods such as spectroscopy methods according to the component included, thereby the amount contained by the per unit weight of the polyamide resin composition is obtained. In addition, the amount of the polyamide resin (B1) contained by the per unit weight of the polyamide resin composition under the situation of the organic component or inorganic component including compatibility can be obtained according to the method.

[0150] On the other hand, since the ammonium salt (C) can be extracted with water, a known weight of the polyamide resin composition is extracted for a sufficient time using, for example, a Soxhlet extractor, and the extract is analyzed by, for example, NMR, FT-IR, GC-MS, liquid chromatography, etc., alone or in combination, depending on the components contained, thereby determining the chemical structure of the ammonium salt (C) and the content of the ammonium salt (C) and the content of ammonium ions [B].

[0151] <Content of each ingredient>

[0152] The molded product of the present invention contains 5 to 50 parts by weight of reinforcing fiber (A) relative to a total of 100 parts by weight of reinforcing fiber (A), polyamide resin composition (B) and ammonium salt (C). If the content of reinforcing fiber (A) is less than 5 parts by weight, the mechanical properties, especially bending properties and impact properties of the molded product are reduced. The content of reinforcing fiber (A) is preferably 7 parts by weight or more, more preferably 10 parts by weight or more. On the other hand, if the content of reinforcing fiber (A) exceeds 50 parts by weight, the entanglement of the fibers increases. As a result, due to fiber breakage, the fiber length is shortened, and the bending properties and impact properties are reduced. The content of reinforcing fiber (A) is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, and further preferably 15 parts by weight or less.

[0153] The content of the polyamide resin composition (B) in the molded article of the present invention is 40 to 94.9 parts by weight relative to a total of 100 parts by weight of the reinforcing fibers (A), the polyamide resin composition (B) and the ammonium salt (C). When the content of the polyamide resin composition (B) is less than 40 parts by weight, the entanglement of the reinforcing fibers (A) increases, fiber breakage occurs, and the fiber length becomes shorter, and the bending strength and impact properties decrease. The content of the polyamide resin composition (B) is preferably 50 parts by weight or more. On the other hand, when the content of the polyamide resin composition (B) exceeds 94.9 parts by weight, the content of the carbon fiber (A) and the ammonium salt (C) decreases relatively, so the reinforcing effect brought by the fiber becomes weak, and the mechanical properties, especially the bending properties and impact properties decrease. The content of the polyamide resin composition (B) is preferably 85 parts by weight or less, and more preferably 80 parts by weight or less.

[0154] <Other ingredients (D)>

[0155] The molded article of the present invention may contain other components (D) in addition to the above-mentioned (A) to (C) within the scope not impairing the purpose of the present invention. Examples of other components (D) include thermosetting resins, petroleum resins, flame retardants, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, coloring inhibitors, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, foaming agents, foaming agents, or coupling agents.

[0156] Here, as other components (D), in order to ensure higher fiber dispersibility, epoxy resin, phenol resin, terpene resin may be included, and more than two of them may be included. As component (D), it is preferably a material with high affinity to polyamide resin composition (B). By selecting a component (D) with high affinity to polyamide resin composition (B), it is possible to efficiently be compatible with polyamide resin composition (B) during injection molding, so that the dispersibility of carbon fiber (A1) and organic fiber (A2) can be further improved.

[0157] Component (D) is appropriately selected according to the combination with the molding temperature of the polyamide resin composition (B). For example, when the molding temperature is in the range of 150°C to 270°C, a terpene resin is preferably used. When the molding temperature is in the range of 270°C to 320°C, a phenol resin is preferably used.

[0158] The heating loss of component (D) at 10°C / min heating (in air) at the molding temperature is preferably 10% by weight or less. More preferably, it is 5% by weight or less, and further preferably, it is 3% by weight or less. When such a heating loss is 10% by weight or less, the generation of decomposition gas can be suppressed when injection molding is performed with the polyamide resin composition (B), and the generation of voids can be suppressed during molding. In addition, the generation of gas can be suppressed, especially in molding at high temperatures.

[0159] In addition, the so-called heating loss in the present invention means that the weight of the component (D) before heating is set to 100%, and the weight loss rate of the component (D) before and after heating under the above heating conditions can be obtained by the following formula. The weight before and after heating can be obtained by measuring the weight at the molding temperature by thermogravimetric analysis (TGA) using a platinum sample pan in an air atmosphere at a heating rate of 10°C / min.

[0160] Heating loss [weight %] = {(weight before heating - weight after heating) / weight before heating} × 100

[0161] As terpene resins, for example, polymers or copolymers obtained by polymerizing terpene monomers with aromatic monomers as needed in an organic solvent in the presence of a Friedel-Crafts type catalyst can be cited. In particular, as terpene monomers, α-pinene, β-pinene, dipentene, d-limonene are preferred due to their excellent compatibility with the polyamide resin composition (B), and more preferably, homopolymers of these terpene monomers. In addition, hydrogenated terpene resins obtained by hydrogenating these terpene resins and terpene phenol resins obtained by reacting terpene monomers with phenols in the presence of a catalyst can also be used. Here, as phenols, substances having 1 to 3 substituents selected from at least one of an alkyl group, a halogen atom, and a hydroxyl group on the benzene ring of phenol are preferably used. Among them, phenol and cresol are preferred. Among them, hydrogenated terpene resins are preferred due to their excellent compatibility with the polyamide resin composition (B).

[0162] In addition, the glass transition temperature of the terpene resin is not particularly limited, but is preferably 30 to 100° C. If the glass transition temperature is 30° C. or higher, the handleability of the component (D) during molding is excellent. In addition, if the glass transition temperature is 100° C. or lower, the fluidity of the component (D) during molding can be appropriately suppressed, thereby improving the moldability.

[0163] The content of component (D) in the molding material of the present invention is preferably 1 to 20 parts by weight relative to a total of 100 parts by weight of the reinforcing fiber (A), the polyamide resin composition (B) and the ammonium salt. When the content of component (D) is less than 1 part by weight, the dispersibility of the carbon fiber (A1) and the organic fiber (A2) during injection molding is reduced. The content of component (D) is preferably 2 parts by weight or more, preferably 4 parts by weight or more. On the other hand, when the content of component (D) exceeds 20 parts by weight, the bending properties and impact properties of the molded product are reduced. Preferably it is 15 parts by weight or less, more preferably 12 parts by weight or less, and further preferably 10 parts by weight or less.

[0164] The molding material in the present invention is not particularly limited, but specific shapes include: Figure 1 to Figure 4 A columnar body with a cross section as shown. In such a columnar body, it is preferred that the carbon fiber (A1) and the organic fiber (A2) are arranged almost parallel to the axial direction of the columnar body, and the length of the carbon fiber (A1) and the organic fiber (A2) is substantially the same as the length of the molding material. By making the length of the fiber substantially the same as the length of the molding material, it is easy to control the fiber length of the carbon fiber (A1) and the organic fiber (A2) in the molded product manufactured using it, and in addition, it can be made longer, so that a molded product with better mechanical properties can be obtained. In addition, the so-called "almost parallel arrangement" means that the axis of the long axis of the fiber bundle containing carbon fiber (A1) and organic fiber (A2) points to the same direction as the axis of the long axis of the molding material, and the deviation of the angles between the axes is preferably less than 20°, more preferably less than 10°, and further preferably less than 5°. The so-called length of the molding material is the length of the orientation direction of the fiber bundle in the molding material, and in the case of the above-mentioned columnar body, it is the length of the long axis direction of the columnar body. In addition, the term "substantially the same length" means that the fiber bundles are not intentionally cut inside the molding material, or that the molding material does not substantially contain fiber bundles significantly shorter than the total length of the molding material. In particular, the amount of fiber bundles shorter than the total length of the molding material is not limited, but the content of fiber bundles having a length of 50% or less of the total length of the molding material is preferably 30% by mass or less, more preferably 20% by mass or less in all the fiber bundles. More preferably, the content of fiber bundles having a length of 85% or more of the total length of the molding material is preferably 80% by mass or more, more preferably 90% by mass or more.

[0165] The molding material preferably has almost the same cross-sectional shape continuously along a certain length in the longitudinal direction. The length of the molding material in the longitudinal direction is in the range of 3 mm to 7 mm. In the case of less than 3 mm, the reinforcing effect of the fiber is lacking. In other words, when molding is performed using a molding material less than 3 mm, the weight-average fiber length of the organic fibers in the resulting molded product cannot be made sufficiently long, so the impact characteristics are poor. The molding material is preferably 4 mm or more, more preferably 5 mm or more. On the other hand, when the molding material exceeds 7 mm, the moldability during injection molding is reduced. In other words, when the length of the molding material exceeds 7 mm, the molding material is long, so the molding material does not bite in the injection molding machine, which is not preferred.

[0166] The molding material in the present invention preferably has a fiber bundle containing carbon fiber (A1) and organic fiber (A2) as a continuous fiber bundle in a resin composition containing a polyamide resin composition (B) and an ammonium salt (C). In other words, it is preferably configured with a polyamide resin composition (B) and an ammonium salt (C) on the outside of the fiber bundle. In the polyamide resin composition (B), component (D) may be included. In addition, a composite fiber bundle (E) in which component (D) is filled between each single fiber of the above-mentioned fiber bundle can be constituted, and a polyamide resin composition (B) and an ammonium salt (C) are configured on its outside. The composite fiber bundle (E) is formed by impregnating the fiber bundle with component (D), and is a state in which carbon fiber (A1) and organic fiber (A2) are dispersed like an island in the sea of ​​component (D).

[0167] The molding material in the present invention preferably has a core-sheath structure in which the fiber bundle or composite fiber bundle (E) is coated with the polyamide resin composition (B) and the ammonium salt (C). The polyamide resin composition (B) and the ammonium salt (C) forming the sheath structure may further contain other components as needed to form a polyamide resin composition composition. Here, the so-called "coated structure" refers to a structure in which a composition containing the polyamide resin composition (B) and the ammonium salt (C) (hereinafter, sometimes referred to as "polyamide resin composition (B)" in the case of the composition) is arranged on the surface of the fiber bundle or composite fiber bundle (E) and bonded.

[0168] The component (D) contained in the molding material of the present invention is often of low molecular weight, and is often a solid or liquid that is generally brittle and easily broken at room temperature. By including the polyamide resin composition (B) on the outside of the composite fiber bundle (E), the high molecular weight polyamide resin composition (B) protects the composite fiber bundle (E), and the crushing and scattering of the component (D) caused by the impact and friction during the transportation and operation of the molding material can be suppressed, and the shape of the molding material can be maintained. From the viewpoint of operability, the molding material of the present invention preferably maintains the above shape until it is provided for molding.

[0169] The composite fiber bundle (E) and the polyamide resin composition (B) and the ammonium salt (C) may be in a state where the polyamide resin composition (B) and the ammonium salt (C) partially penetrate into a part of the composite fiber bundle (E) near the boundary and are compatible, or may be in a state where the polyamide resin composition (B) and the ammonium salt (C) are impregnated in the composite fiber bundle (E).

[0170] The molding material of the present invention preferably has carbon fibers (A1) and organic fibers (A2) offset in the cross section of the fiber bundle. Here, the so-called fiber bundle cross section refers to a cross section that is perpendicular to the fiber length direction of the fiber bundle. In the cross section of the fiber bundle, the carbon fibers (A1) and the organic fibers (A2) are offset, so that the entanglement of the carbon fibers (A1) and the organic fibers (A2) during molding can be suppressed, and a molded product in which the carbon fibers (A1) and the organic fibers (A2) are evenly dispersed can be obtained. Therefore, the impact properties of the molded product can be further improved. Here, the so-called "offset" in the present invention means that in the cross section of the fiber bundle, the carbon fibers (A1) and the organic fibers (A2) are not equally present in all areas, but are partially biased.

[0171] For example, Figure 1 As shown in FIG. 1 , in the cross section of the fiber bundle in the polyamide resin composition (B) and the ammonium salt (C) 3, the carbon fiber (A1) 1 contains the organic fiber (A2) 2, Figure 2 As shown in the figure, the so-called core-sheath structure is a structure in which the organic fiber (A2) 2 encloses the carbon fiber (A1) 1. Figure 3 The structure in which one bundle of carbon fibers (A1) and two bundles of organic fibers (A2) exist separately in a state of being separated by a certain boundary in the cross section of the fiber bundle as shown in the figure is a scheme of "biasing" in the present invention. In addition, the so-called "inner wrapping" in the present invention refers to a scheme in which the carbon fibers (A1) are arranged in the core and the organic fibers (A2) are arranged in the sheath, a scheme in which the organic fibers (A2) are arranged in the core and the carbon fibers (A1) are arranged in the sheath, etc. Figure 3 In the embodiment shown in FIG. 1 , at least a portion of each of the carbon fibers (A1) and the organic fibers (A2) in the fiber bundle cross section is in contact with the polyamide resin composition (B) and the ammonium salt (C) 3 of the outer layer. In this case, the embodiment in which the carbon fibers (A1) or the organic fibers (A2) are in contact with the polyamide resin composition (B) and the ammonium salt (C) 3 also includes the following: Figure 4 As shown, the carbon fiber (A1) or the organic fiber (A2) is in contact with the polyamide resin composition (B) and the ammonium salt (C) 3 via the component (D).

[0172] In addition, in the present invention, as a method for confirming the bias of carbon fibers (A1) and organic fibers (A2) in a fiber bundle, for example, a method of observing a cross section perpendicular to the fiber length direction of the molding material using an optical microscope set to a magnification of 300 times, and performing image processing and analysis of the obtained microscope image can be cited.

[0173] As a method for offsetting the carbon fiber (A1) and the organic fiber (A2) in the cross section of the fiber bundle, there can be cited a method of preparing the above-mentioned molding material by paralleling the carbon fiber (A1) bundle and the organic fiber (A2) bundle. By paralleling the bundles to prepare the molding material, the carbon fiber (A1) and the organic fiber (A2) exist as independent fiber bundles, which can be offset. If the number of single fibers in the carbon fiber (A1) bundle and the organic fiber (A2) bundle used is large, the bundle can be made large, and if the number of single fibers is small, the bundle can be made small, and the size of the bundle can be changed to make it offset.

[0174] The carbon fiber (A1) is not particularly limited, but preferably uses a fiber bundle having 100 to 350,000 carbon fibers, and more preferably uses a fiber bundle having 20,000 to 100,000 carbon fibers from the viewpoint of productivity. On the other hand, when polyester fibers or liquid crystal polyester fibers are used as the organic fibers (A2), there is no particular limitation, but preferably uses a fiber bundle having 1 to 2,000 carbon fibers, and more preferably uses a fiber bundle having 10 to 1,000 carbon fibers, and still more preferably uses a fiber bundle having 30 to 700 carbon fibers from the viewpoint of suppressing entanglement between fibers in the molded article and productivity.

[0175] By molding using the molding material, it is possible to obtain a molded product having excellent dispersibility and moldability of the carbon fibers (A1) and the organic fibers (A2) and excellent bending strength and impact properties.

[0176] Next, a method for producing the above-mentioned molding material will be described. The molding material in the present invention can be obtained, for example, by the following method.

[0177] First, the roving of carbon fiber (A1) and the roving of organic fiber (A2) are combined in parallel with respect to the fiber length direction to produce a fiber bundle having carbon fiber (A1) and organic fiber (A2). Next, the molten component (D) is impregnated into the fiber bundle to produce a composite fiber bundle (E). Furthermore, the composite fiber bundle (E) is introduced into an impregnation die filled with a composition comprising a molten polyamide resin composition (B) and an ammonium salt (C), so that the polyamide resin composition (B) and the ammonium salt (C) are coated on the outside of the composite fiber bundle (E) and are extracted through a nozzle. A method of obtaining a molding material by granulating into a specified length after cooling and solidification can be cited. As long as the polyamide resin composition (B) and the ammonium salt (C) are at least arranged on the outside of the composite fiber bundle (E), they can be impregnated in the fiber bundle.

[0178] The molding material prepared by the above method, in which the composite fiber bundle (E) is coated with a polyamide resin composition (B) and an ammonium salt (C), and the particles (excluding carbon fiber (A1) and organic fiber (A2)) containing the polyamide resin composition (B) are mixed with particles to obtain a molding material mixture. Thus, the content of carbon fiber (A1) and organic fiber (A2) in the molded product can be easily adjusted. In addition, the so-called particle blending, unlike melt mixing, refers to stirring / mixing a variety of materials at a temperature at which the resin component is not melted to form a substantially uniform state. In the case of using a particle-shaped molding material, injection molding, extrusion molding, etc. are mainly preferably used.

[0179] Next, a method for producing the molded article of the present invention will be described.

[0180] By using the molding material in the present invention as described above for molding, a molded product with excellent moldability, bending properties, impact properties and appearance quality can be obtained. As a molding method, a molding method using a mold is preferred, and various molding methods such as injection molding, extrusion molding, and compression molding can be used. In particular, by using a molding method using an injection molding machine, a continuously stable molded product can be obtained. As injection molding conditions, there are no special regulations, for example, the injection time is preferably 0.5 seconds to 10 seconds, and more preferably 2 seconds to 10 seconds. The back pressure is preferably 0.1MPa or more, more preferably 1MPa or more, more preferably 2MPa or more, and most preferably 3MPa or more. In addition, the upper limit is preferably 50MPa or less, more preferably 30MPa or less, more preferably 20MPa or less, and most preferably 10MPa or less. The injection speed is preferably 1mm / s to 200mm / s, more preferably 10mm / s to 150mm / s, and more preferably 20mm / s to 100mm / s. The screw speed is preferably 10 rpm to 200 rpm, more preferably 30 rpm to 150 rpm, and further preferably 50 rpm to 100 rpm. The holding pressure is preferably 1 MPa to 50 MPa, and more preferably 1 MPa to 30 MPa. The holding time is preferably 1 second to 20 seconds, and more preferably 5 seconds to 20 seconds. The barrel temperature is preferably 200°C to 320°C, and the mold temperature is preferably 20°C to 100°C. Here, the barrel temperature refers to the temperature of the part where the molding material of the injection molding machine is heated and melted, and the mold temperature refers to the temperature of the mold into which the resin used to make a specified shape is injected. By appropriately selecting these conditions, especially the injection time, back pressure and mold temperature, the fiber length of carbon fibers and organic fibers such as carbon fibers in the molded product can be easily adjusted.

[0181] The molded article of the present invention obtained as described above is excellent in moldability, and is excellent in mechanical properties, particularly flexural strength, impact properties, and appearance quality.

[0182] Example

[0183] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to the description of these Examples. First, the evaluation methods of various properties used in the present Examples will be described.

[0184] (1) Determination of weight-average fiber length

[0185] On a hot stage set to a temperature (e.g., 200 to 300° C.) at which the organic fiber (A2) does not melt but only the polyamide resin composition (B) melts, a 0.5 cm square test piece cut from an ISO dumbbell test piece obtained by each embodiment and comparative example is heated in a state sandwiched between cover glasses without applying excessive pressure, and the fibers are made into a film so that the fibers are evenly dispersed. The film in which the carbon fiber (A1) and the organic fiber (A2) are evenly dispersed is observed using an optical microscope (50 to 200 times). The fiber lengths of 1000 randomly selected carbon fibers (A1) and 1000 randomly selected organic fibers (A2) are measured respectively, and the weight-average fiber length is calculated by the following formula.

[0186] Average fiber length = Σ(Mi 2 ×Ni) / Σ(Mi×Ni)

[0187] Mi: Fiber length (mm)

[0188] Ni: The number of fibers with a fiber length of Mi.

[0189] (2) Determination of flexural strength and flexural modulus of molded products, and flexural modulus when water is absorbed

[0190] Regarding the ISO dumbbell test pieces obtained by each embodiment and comparative example, according to ISO 178:2010, Amd.1:2013, a 3-point bending test fixture (indenter radius 5 mm) was used to set the fulcrum distance to 64 mm, and the bending strength and bending modulus were measured under the test conditions of a test speed of 2 mm / min. As a testing machine, "Instron (registered trademark)" universal testing machine 5566 type (manufactured by Instron Co., Ltd.) was used. The measurement was carried out 3 times, and the average value was calculated as the bending strength and bending modulus of each embodiment and comparative example. At this time, in the calculation of the bending modulus, it is calculated from the stress gradient of the specified strain range (0.05~0.25%).

[0191] In addition, about the water absorption ISO type dumbbell test piece mentioned later, the bending elastic modulus was measured in the same manner as above.

[0192] (3) Charpy impact strength measurement of molded products

[0193] The parallel part of the ISO dumbbell test piece obtained by each example and comparative example was cut out, and a V-notched Charpy impact test was performed according to ISO179 using a C1-4-01 tester manufactured by Tokyo Test Machinery Co., Ltd. The measurement was performed 5 times, and the average value was used as the impact strength (kJ / m 2 ) and calculated.

[0194] (4) Evaluation of fiber dispersion of molded products

[0195] The number of undispersed carbon fiber bundles (CF bundles) on the front and back surfaces of the 80 mm × 80 mm × 3 mm thick test pieces obtained by each embodiment and comparative example was visually counted. The evaluation was performed on 50 molded products, and the fiber dispersibility was determined based on the following criteria for the total number of CF bundles, with A and B being considered acceptable.

[0196] A: less than 1 undispersed CF bundle

[0197] B: The number of undispersed CF bundles is 1 or more and less than 3

[0198] C: The number of undispersed CF bundles is 3 or more.

[0199] (5) Liquidity evaluation

[0200] The fiber-reinforced polyamide resin composition pellets were vacuum dried at 80°C for 12 hours, and injection molded using an injection molding machine (J110AD manufactured by Japan Steel Works) at a barrel temperature of the melting point of the polyamide resin + 15°C, a mold temperature of 80°C, a shot speed of 60 mm / sec, and an injection pressure of 60 MPa using a mold of 10 mm in width × 150 mm in length × 1.0 mm in length to produce a rod flow test piece of 10 mm in width × 1.0 mm in thickness. The rod flow length under holding pressure 0 was measured 5 times, and the average value was obtained to evaluate the fluidity. It was shown that the longer the flow length, the better the fluidity.

[0201] (6) Morphological observation

[0202] The center of the cross-sectional direction of the JIS-5A dumbbell-shaped test piece or the bending test piece obtained by injection molding was cut into 1-2 mm squares, stained with ruthenium tetroxide, and the resin (B2) having a reactive functional group was stained. The test piece was cut at -196°C by an ultrathin slicer to obtain ultrathin slices with a thickness of less than 0.1 μm (about 80 nm). The slices were observed with a transmission electron microscope. The number average particle size (Xn) was obtained by randomly extracting more than 400 particles from the obtained image, and the particle size distribution was analyzed using the image analysis software "Scion Image" manufactured by Scion Corporation, and the particle size distribution was analyzed and obtained by the following formula.

[0203] Number average particle size (Xn) = Σ(Xi×ni) / Σni

[0204] Xi; particle size

[0205] ni; number of particles that match the particle size (Xi)

[0206] (i=1,2,3,···,n)

[0207] The number average particle size of particles formed from resin (B2) was calculated from an image magnified 10,000 times, and the number average particle size of fine particles in particles formed from resin (B2) was calculated from an image magnified 35,000 times. The number average particle size of particles formed from resin (B2), the presence or absence of fine particles of 1 to 100 nm of compound (B3), and the presence or absence of fine particles exceeding 300 nm were confirmed.

[0208] Furthermore, the area ratio occupied by the compound (B3) was determined by analyzing the area of ​​the resin (B2) and the area occupied by the compound (B3) using the image analysis software "Scion Image" manufactured by Scion Corporation using a transmission electron microscope and the above image magnified 35,000 times, and the result was determined by the following formula.

[0209] Sn=Sp / (Sa2+Sp)

[0210] Sn: Area ratio of the compound (B3) in the particles formed by the resin (B2)

[0211] Sa2: Area occupied by resin (B2)

[0212] Sp; area occupied by compound (B3).

[0213] (7) Determination of water absorption

[0214] The ISO dumbbell test pieces obtained in each example and comparative example were weighed after being left to stand in a constant temperature room at 23°C and 50% humidity for 24 hours, and then left to stand in an environment of 80°C × 95% RH for 24 hours. Then, the weight of the water-absorbent ISO dumbbell test piece was wiped off, and the water absorption rate of the ISO dumbbell test piece before and after water absorption was calculated.

[0215] <Carbon Fiber (A1)>

[0216] Reference Example 1: Preparation of carbon fiber (A1)

[0217] The copolymer with polyacrylonitrile as the main component was spun, calcined, and surface oxidized to obtain a total of 24,000 single fibers with a single fiber diameter of 7 μm, a mass per unit length of 1.6 g / m, and a specific gravity of 1.8 g / cm 3, a continuous carbon fiber having a surface oxygen concentration ratio [O / C] of 0.2. The continuous carbon fiber had a tow tensile strength of 4,880 MPa and a tow tensile elastic modulus of 225 GPa. Next, a sizing agent mother solution was prepared in which glycerol polyglycidyl ether, a multifunctional compound, was dissolved in water in an amount of 2% by weight, and the sizing agent was applied to the carbon fiber by an impregnation method and dried at 230°C. The carbon fiber obtained in this way had a sizing agent adhesion amount of 1.0% by weight.

[0218] Reference Example 2: Preparation of dendritic polyester (C-3)

[0219] In a 500 mL reaction container equipped with a stirring blade and a distillation tube, 51.93 g (0.38 mol) of p-hydroxybenzoic acid, 19.1 g (0.10 mol) of 4,4'-dihydroxybiphenyl, 5.86 g (0.035 mol) of terephthalic acid, 21.2 g (0.10 mol) of trimesic acid, 5.55 g (0.045 mol) of benzoic acid, 11.3 g (0.059 mol) of polyethylene terephthalate having an intrinsic viscosity of about 0.6 dl / g, and 65.3 g (1.10 equivalents of the total phenolic hydroxyl groups) of acetic anhydride were added, and the mixture was reacted at 150° C. for 1.5 hours with stirring in a nitrogen atmosphere. After the temperature was raised to 290°C over 3 hours, the pressure was reduced to 1.0 mmHg (133 Pa) over 30 minutes while the polymerization temperature was maintained at 290°C. When the stirring torque reached 2.5 kg·cm, the polymerization reaction was stopped and the contents were discharged into water. The obtained dendritic polyester (C-1) was dried by heating at 110°C for 4 hours, crushed with a stirrer, and washed with ethanol and deionized water. Then, it was vacuum dried at 110°C for 24 hours using a vacuum heating dryer to obtain a powdery dendritic polyester (C-3).

[0220] <Organic fiber (A2)>

[0221] (A2-1): Liquid crystal polyester fiber ("Sibelus" (registered trademark) 1700T-288f manufactured by Toray Industries, Ltd., strength: 23.5 cN / dtex, melting point 330°C) was used.

[0222] (A2-2): Polyester fiber (manufactured by Toray Industries, Ltd., "Tetron (registered trademark)" 2200T-480-705M, single fiber fineness: 4.6 dtex, melting point: 260°C) was used.

[0223] (A2-3): Polyphenylene sulfide fiber (Toray Industries, Inc., "Torucon" (registered trademark) 400T-100-190, single fiber fineness 4.0 dtex, melting point 285°C) was used.

[0224] (A2-4): Polytetrafluoroethylene fiber (Toyofluon (registered trademark) 440T-60F-S290-M190 manufactured by Toray Industries, Ltd., single fiber fineness 7.3 dtex, melting point 327°C) was used.

[0225] <Polyamide resin composition (B)>

[0226] Polyamide resin (B1a)

[0227] (B1a-1): Nylon 6 resin having a melting point of 225°C and a relative viscosity of 2.75 at 0.01 g / ml in 98% sulfuric acid.

[0228] (B1a-2): Nylon 66 resin having a melting point of 265°C and a relative viscosity of 3.60 at 0.01 g / ml in 98% sulfuric acid.

[0229] (B1a-3): Nylon 610 resin having a melting point of 225°C and a relative viscosity of 2.70 at 0.01 g / ml in 98% sulfuric acid.

[0230] Polyamide resin (B1b)

[0231] (B1b-1): Nylon 610 resin having a melting point of 225°C and a relative viscosity of 2.70 at 0.01 g / ml in 98% sulfuric acid.

[0232] (B1b-2): Nylon 11 resin having a melting point of 190°C and a relative viscosity of 2.55 at 0.01 g / ml in 98% sulfuric acid.

[0233] (B1b-3): Nylon 12 resin having a melting point of 180°C and a relative viscosity of 2.55 at 0.01 g / ml in 98% sulfuric acid.

[0234] Resin with reactive functional groups (B2)

[0235] (B2-1): Glycidyl methacrylate-modified polyethylene copolymer "Bondo Form (registered trademark) BF-7L" (manufactured by Sumitomo Chemical Co., Ltd.).

[0236] (B2-2): Glycidyl methacrylate-modified polyethylene copolymer "Bondo Form (registered trademark) BF-7M" (manufactured by Sumitomo Chemical Co., Ltd.).

[0237] (B2-3): Maleic anhydride-modified ethylene-1-butene copolymer "TAFMAR (registered trademark) MH7020" (manufactured by Mitsui Chemicals, Inc.).

[0238] (B2-4): Ethylene-methacrylic acid-zinc methacrylic acid copolymer "Hydron (registered trademark) 1706" (manufactured by Mitsui Chemical Co., Ltd.).

[0239] (B2-5): Contains Oxazoline-based reactive polystyrene "EPOCLOSURES (registered trademark) RPS-1005" (manufactured by Nippon Shokubai Co., Ltd.).

[0240] <Ammonium salt (C) or flow improver (C) used in comparative examples (C-2 and C-3)>

[0241] (C-1): Diammonium adipate (manufactured by Fujifilm Wako Junyu Co., Ltd.)

[0242] (C-2): Adipic acid (manufactured by Fujifilm and Wako Junyu Co., Ltd.)

[0243] (C-3): Dendritic polyester obtained in Reference Example 2

[0244] <Ingredient (D)>

[0245] (D-1)

[0246] A solid terpene phenol resin ("Microace" (registered trademark) K125 manufactured by Yashara Chemical Co., Ltd., softening point 125° C.) was used.

[0247] (Example 1)

[0248] A long fiber reinforced resin pellet production apparatus was used in which a coating die for a wire coating method was provided at the tip of a TEX-30α twin screw extruder (screw diameter 30 mm, L / D=32) manufactured by The Nippon Steel Corporation. The extruder barrel temperature was set to 270° C., and the polyamide resin composition (B1-1), resin (B2-1) and ammonium salt (C-1) shown above were supplied from a main hopper and melt kneaded at a screw speed of 200 rpm. A fiber bundle composed of carbon fiber (A1) and organic fiber (A2) was supplied to a die orifice (3 mm in diameter) from which a composition containing molten polyamide resin (B1-1), resin (B2-1) and ammonium salt (C-1) was discharged, so that the periphery of carbon fiber (A1) and organic fiber (A2) was continuously coated with the composition containing molten polyamide resin (B1-1), resin (B2-1) and ammonium salt (C-1). In the internal cross section of the composite fiber bundle (E) at this time, the carbon fibers (A1) and the organic fibers (A2) are offset. Figure 3As shown, at least a portion of each of the carbon fiber (A1) and the organic fiber (A2) is in contact with a composition comprising a molten polyamide resin (B1-1), a resin (B2-1) and an ammonium salt (C-1). After the obtained tow is cooled, it is cut into pellets of 7 mm in length with a cutter to prepare long-fiber pellets. At this time, the pulling speed is adjusted so that the reinforcing fiber (A) becomes 25 parts by weight relative to a total of 100 parts by weight of (A) to (C) (80 parts by weight of the carbon fiber (A1) and 20 parts by weight of the organic fiber (A2) relative to 100 parts by weight of the reinforcing fiber (A)). The lengths of the carbon fiber (A1) and the organic fiber (A2) of the obtained long-fiber pellets are substantially the same as the pellet length.

[0249] The long fiber pellets obtained in this way were injection molded using an injection molding machine (J110AD manufactured by Nippon Steel Works, Ltd.) under the conditions of injection time: 2 seconds, back pressure 5 MPa, holding pressure: 40 MPa, holding time: 10 seconds, injection speed 30 mm / s, screw speed 80 rpm, barrel temperature: 270°C, and mold temperature: 80°C, thereby producing ISO type dumbbell test pieces (A1 type) and 80 mm×80 mm×3 mm test pieces as molded products. Here, the barrel temperature refers to the temperature of the portion where the molding material of the injection molding machine is heated and melted, and the mold temperature refers to the temperature of the mold into which the resin used to form a specified shape is injected. The obtained test piece (molded product) was left to stand for 24 hours in a constant temperature and humidity chamber adjusted to a temperature of 23°C and 50% RH for property evaluation. The evaluation results evaluated by the above method are summarized in Table 1.

[0250] (Examples 2 to 5, 7 to 17, 31 to 35, 41 to 54, 56)

[0251] Molded products were produced and evaluated in the same manner as in Example 1 (in Example 13, the cylinder temperature was set to 280° C.), except that the composition ratio or the fiber type used was changed as described in Tables 1 and 2. The evaluation results are summarized in Tables 1, 2, 3, 4, and 5.

[0252] (Example 6)

[0253] The same procedure as in Example 1 was carried out except that the molding back pressure during injection molding was changed to 10 MPa to produce a molded article and evaluate it. The evaluation results are summarized in Table 1.

[0254] (Examples 18 to 30, 38 to 40, 55, 57)

[0255] A long fiber reinforced resin pellet manufacturing apparatus was used in which a coating die for a wire coating method was provided at the front end of a TEX-30α twin-screw extruder (screw diameter 30 mm, L / D=32) manufactured by Nippon Steel Works, Ltd. The extruder barrel temperature was set to 270°C, and the polyamide resin composition (B1-1), resin (B2-1) and ammonium salt (C-1) shown above were supplied from the main hopper and melt-kneaded at a screw speed of 200 rpm. The component (D-1) melted by heating at 200°C is adjusted in discharge amount to 8 parts by weight relative to 100 parts by weight of the total of (A) to (C), and is applied to a fiber bundle made of carbon fibers (A1) and organic fibers (A2) to prepare a composite fiber bundle (E). The composite fiber bundle (E) is then supplied to a die (3 mm in diameter) that discharges a composition containing melted polyamide resin (B1-1), resin (B2-1) and ammonium salt (C-1), so that the carbon fibers (A1) and organic fibers (A2) are continuously coated with the composition containing melted polyamide resin (B1-1), resin (B2-1) and ammonium salt (C-1). With respect to the internal cross-section of the composite fiber bundle (E) at this time, the carbon fibers (A1) and the organic fibers (A2) are offset. The offset state is as follows. Figure 3 As shown in the figure, at least a part of each of the carbon fiber (A1) and the organic fiber (A2) is in contact with a composition containing a molten polyamide resin (B1-1), a resin (B2-1) and an ammonium salt (C-1). After the obtained tow is cooled, it is cut into a pellet length of 7 mm with a cutter to prepare a long fiber pellet. A molded article is produced in the same manner as in Example 1 and evaluated. The evaluation results are summarized in Tables 2, 3, 4 and 5.

[0256] (Example 36)

[0257] The evaluation results are summarized in Table 3, except that the molding back pressure during injection molding was changed to 7 MPa, a molded article was produced in the same manner as in Example 1 and evaluated.

[0258] (Example 37)

[0259] The evaluation results are summarized in Table 4, and are shown in Table 4.

[0260] (Comparative Examples 1 to 7, 9 to 11)

[0261] A molded article was produced and evaluated in the same manner as in Example 1 except that the composition was changed as shown in Table 6. Table 6 summarizes the evaluation results.

[0262] (Comparative Example 8)

[0263] The molded products were produced and evaluated in the same manner as in Example 1 except that the molding back pressure during injection molding was changed to 40 MPa. The evaluation results are summarized in Table 6.

[0264]

[0265]

[0266]

[0267]

[0268]

[0269]

[0270] The molded products of the examples show high bending strength and impact properties, and the inclusion of ammonium salt (C) results in excellent fluidity and excellent fiber dispersibility. Examples 5 to 51, 53 to 57 show particularly high impact strength of the molded products by virtue of the reinforcing fiber (A) containing carbon fiber (A1) and organic fiber (A2). In addition, Examples 31 to 51, 56 and 57 in which the polyamide resin (B1) contains polyamide resin (B1a) and polyamide resin (B1b) can reduce the water absorption of the molded products, thereby suppressing the reduction in rigidity during water absorption, and further showing excellent fiber dispersibility and high impact properties. In addition, in the case of Examples 6, 36 and 37 in which the molding back pressure is changed, the same excellent effects as above are also shown. Furthermore, Examples 18 to 30, 38 to 40, 55 and 57 containing component (D) show particularly high bending strength and impact properties because the carbon fiber (A1) and organic fiber (A2) have excellent dispersibility. Even in Examples 25 to 30 and 46 to 51 in which the type of organic fiber is changed, high flexural strength and impact properties are exhibited. The inclusion of the ammonium salt (C) and the polyamide resin (B1b) can reduce the water absorption of the molded article and suppress the reduction in rigidity during water absorption, and can further exhibit excellent fluidity and excellent fiber dispersibility.

[0271] On the other hand, since Comparative Examples 1 and 6 did not contain the ammonium salt (C), the fluidity and fiber dispersibility of the molded product were poor. Since Comparative Example 2 did not contain the resin (B2), the impact strength was poor. Since Comparative Example 3 contained a small amount of carbon fiber (A1), the reinforcement effect was poor, and the mechanical properties of the molded product were reduced. Since Comparative Examples 4 and 5 contained excessive amounts of carbon fiber (A1) or organic fiber (A2), respectively, breakage caused by contact between fibers occurred, and the remaining fiber length became short, resulting in low impact strength.

[0272] In addition, since Comparative Example 7 contains an excessive amount of ammonium salt (C), the plasticization of the polyamide resin composition (B) is promoted, resulting in poor mechanical properties. Since Comparative Example 8 sets the back pressure during molding to a high level, the remaining fiber length of the reinforcing fiber (A) is shortened, resulting in low mechanical properties. Since Comparative Example 9 does not control the number average particle size of the resin (B2) to be in the range of 10 to 1000 nm, the impact properties are reduced. Since Comparative Example 10 does not contain an ammonium salt (C) and only adipic acid is used, the decomposition of the polyamide resin composition (B) is promoted and the mechanical properties are poor. Since Comparative Example 11 uses a flow modifier that is not an ammonium salt (C), the fiber dispersibility is poor.

[0273] Explanation of symbols

[0274] 1 Carbon fiber (A1)

[0275] 2Organic fiber (A2)

[0276] 3. Polyamide resin composition (B) and ammonium salt (C)

[0277] 4. Ingredient (D).

Claims

1. A fiber-reinforced polyamide resin composition molded product, characterized in that: Include: Reinforcement fiber A 5-50 parts by weight, Polyamide resin composition B 40 to 94.9 parts by weight, and 0.1 to 10 parts by weight of an ammonium salt C formed by an aliphatic dicarboxylic acid having 6 to 12 carbon atoms and ammonia, wherein the ammonium salt C is R(COO - )2·(NH4 + )2, wherein R is a divalent aliphatic group having 4 to 10 carbon atoms, The weight average fiber length Lwa1 of the reinforcing fiber A is 0.4 to 7 mm, and the polyamide resin composition B is composed of a polyamide resin B1, a resin B2 having a reactive functional group, and a compound B3 generated by a reaction between the polyamide resin B1 and the resin B2, wherein the resin B2 is dispersed in particles having a number average particle size of 10 to 1,000 nm.

2. The fiber-reinforced polyamide resin composition molded article according to claim 1, wherein the polyamide resin B1 contained in the polyamide resin composition B forms a continuous phase, the resin B2 forms a dispersed phase, and the dispersed phase contains fine particles having a particle size of 1 to 100 nm formed of the compound B3. 3 . The fiber-reinforced polyamide resin composition molded article according to claim 2 , wherein the area ratio of the fine particles formed from the compound B3 in the particles formed from the resin B2 is 20% or more.

4. The fiber-reinforced polyamide resin composition molded article according to any one of claims 1 to 3, wherein the resin B2 is a polymer having an amino group, a carboxyl group, a metal salt of a carboxyl group, an epoxy group, an acid anhydride group and A resin having at least one reactive functional group in an oxazoline group. 5 . The fiber-reinforced polyamide resin composition molded article according to claim 1 , wherein the resin B2 is a polyolefin resin.

6. The fiber-reinforced polyamide resin composition molded article according to any one of claims 1 to 3, wherein the reinforcing fiber A comprises carbon fibers A1 and organic fibers A2, and the reinforcing fiber A comprises 50 to 99 parts by weight of carbon fibers A1 and 1 to 50 parts by weight of organic fibers A2 per 100 parts by weight of the total of the carbon fibers A1 and the organic fibers A2. 7 . The fiber-reinforced polyamide resin composition molded article according to claim 6 , wherein the weight average fiber length Lwa2 of the organic fibers A2 is 3 to 7 mm.

8. The fiber-reinforced polyamide resin composition molded article according to any one of claims 1 to 3, wherein the polyamide resin B1 is a mixture of a polyamide resin B1a and a polyamide resin B1b, the polyamide resin B1a is selected from polyamide 6 and polyamide 66, and the polyamide resin B1b is one or more selected from polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 1012, polyamide 9T, and a copolymer polyamide containing at least one of them as a constituent component. 9 . The fiber-reinforced polyamide resin composition molded article according to claim 8 , wherein the polyamide resin B1 is a mixture of polyamide 6 resin and polyamide 610 resin.

10. The fiber-reinforced polyamide resin composition molded article according to claim 8, which has a water absorption of 3.0% or less when left in an environment of 80°C x 95% RH for 24 hours. 11 . The fiber-reinforced polyamide resin composition molded article according to claim 6 , wherein the organic fiber A2 is at least one selected from liquid crystal polyester fiber, polyarylene sulfide fiber and fluorine fiber.

Citation Information

Patent Citations

  • Thermoplastic resin composition and molded product comprising the same composition

    JP1999140237A

  • Polyamide resin composition and resin metal complex

    JP2013249363A

  • Carbon fiber-containing resin pellet, manufacturing method of carbon fiber-containing resin pellet

    JP2019151712A

  • Fiber reinforced resin composition, molding material, and method for producing fiber reinforced resin composition

    WO2010107022A1

  • Fiber-reinforced thermoplastic-resin molded article, fiber-reinforced thermoplastic-resin molding material, and method for manufacturing fiber-reinforced thermoplastic-resin molding material

    WO2014098103A1