A method and catalyst for directly converting ethylene into ethylene glycol using oxygen
By using a two-dimensional layered transition metal compound catalyst in the ethylene oxidation reaction, ethylene is converted into ethylene glycol at room temperature, solving the problems of high energy consumption and environmental pollution in traditional processes, and achieving high-efficiency and low-cost ethylene glycol Production.
Patent Information
- Application Number
- CN202111370967.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-18
AI Technical Summary
The existing ethylene glycol production process has problems such as high energy consumption, complex separation of catalysts, difficulty in separation of catalysts and environmental pollution. Especially in ethylene oxidation reaction, traditional processes require high oxygen partial pressure and high temperature, and hydrogen peroxide is costly as an oxidant. And the utilization rate is not high.
Two-dimensional layered transition metal compounds and their hybrid structures are used as catalysts to directly catalyze the conversion of ethylene to glycol at room temperature or even lower temperatures, and oxygen as an oxidant, simplify the process flow and reduce energy consumption.
It has achieved efficient preparation of ethylene glycol, with product selectivity reaching more than 80%, high ethylene conversion rate, mild process conditions, and wide selection of catalysts, which reduces production costs and reduces environmental pollution.
Smart Images

Figure CN116135828B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and a catalyst for efficiently preparing ethylene glycol, and in particular to a method for preparing a two-dimensional layered transition metal compound and a hybrid structure thereof, and application thereof in preparing ethylene glycol by oxidizing ethylene. Background Art
[0002] As an important basic chemical, ethylene glycol has a wide range of uses. It is not only used to produce polyethylene terephthalate (PET), but also used to produce antifreeze, lubricants, plasticizers, surfactants and explosives. At the same time, ethylene glycol is also an important part of the chemical fiber (polyester) industry chain. The growth of the polyester industry in recent years has led to a further increase in the demand for ethylene glycol. It is expected that by 2025, the global demand for ethylene glycol will increase to 37,410 kt. At the same time, according to Chinese customs data, my country's ethylene glycol imports may exceed 10,000 kt. From this point of view, my country's demand for ethylene glycol is still very strong.
[0003] At present, the petroleum route of producing ethylene glycol by hydration of ethylene oxide using ethylene as raw material is the most mature and widely used production route for industrial production of ethylene glycol. The traditional petroleum ethylene production route is generally divided into two steps: first, ethylene and oxygen undergo ethylene oxidation reaction under the action of silver catalyst to produce ethylene oxide. This step needs to be carried out at a higher oxygen partial pressure (1-3MPa) and temperature (200-300℃). Then ethylene oxide is directly hydrated or catalytically hydrated to produce ethylene glycol. Although the direct hydration process does not require a catalyst, it needs to react at a high water ratio (molar ratio of 22-25:1) and a certain temperature (90-100℃) to produce ethylene glycol, which leads to a high water content in ethylene glycol, a complex separation and refining process, and high energy consumption; although catalytic hydration can effectively reduce water consumption, the catalyst in the solution is difficult to separate from the product, affecting the product quality of ethylene glycol.
[0004] In addition, the newly emerging coal-to-ethylene glycol process uses coal as raw material, gasifies it into synthesis gas, and then produces ethylene glycol. There are three main process technology routes: direct synthesis, methanol synthesis, and oxalate hydrogenation. The direct synthesis method is to produce synthesis gas through coal gasification, and then directly synthesize ethylene glycol from the synthesis gas in one step. In the process route of the methanol synthesis method, synthesis gas is used to produce methanol and then ethylene, and ethylene glycol is produced through the ethylene route; the next is the oxalate hydrogenation method, which generally includes seven steps and four reactions to produce ethylene glycol. The coal-based conversion route still faces problems such as lengthy process flow, high energy consumption, large emissions of greenhouse gas CO2 during the process, and high economic costs and environmental pressures.
[0005] In order to shorten the process and reduce production costs, the development of efficient catalysts and catalytic systems to achieve one-step synthesis of ethylene glycol has become a hot topic and difficulty in research. In recent years, based on the oxidation of ethylene, researchers have found that titanium silicon molecular sieves can catalyze the oxidation of ethylene to produce ethylene glycol in one step under the action of hydrogen peroxide (H2O2), which is an environmentally friendly and clean preparation method. However, hydrogen peroxide is expensive, which further increases the preparation cost of ethylene glycol. At the same time, due to the easy decomposition of hydrogen peroxide, its utilization rate is not high. In addition, the introduction of hydrogen peroxide adds challenges to the controlled oxidation of ethylene. From the perspective of economic cost and green chemistry, oxygen is the cheapest oxidant, and it is easy to obtain and will not cause environmental pollution and other problems. The one-step method of directly oxidizing ethylene with oxygen as an oxidant to produce ethylene glycol is one of the most valuable and promising ways to develop. At present, there are no patents or relevant literature reports on the research on the direct catalytic oxidation of ethylene to produce ethylene glycol. Summary of the invention
[0006] Based on the above background technology, the present invention has developed a two-dimensional layered transition metal compound and its hybrid structure, and applied it to the ethylene oxidation reaction for the first time, directly catalytically converting ethylene into ethylene glycol (CH2OH-CH2OH) at room temperature or even lower temperature (-10°C), with the selectivity of ethylene glycol in the product maintained at more than 80%, and the conversion rate of ethylene is relatively high.
[0007] To achieve the above object, the technical solution of the present invention is as follows:
[0008] On the one hand, the present invention provides a method for directly catalytically converting ethylene into ethylene glycol using oxygen: the reaction gas is a mixture of C2H4, O2 and CO or H2, the reaction medium is H2O, the reaction temperature is -10 to 100°C, the reaction pressure is 1 to 50 bar, the reaction time is 1 to 10 hours, the catalyst is at least one of a two-dimensional layered transition metal compound and a hybrid structure thereof, the catalyst dosage is 10 to 100 mg, and the reaction apparatus is a high-pressure reactor with a volume of 50 mL.
[0009] Preferably, the pressure of C2H4 in the reaction gas is 1-20 bar, the pressure of O2 is 0.25-3 bar, and the pressure of CO or H2 is 1-30 bar.
[0010] Preferably, the reaction medium is ultrapure water with a resistivity of 2-40 mL, and more preferably, the amount is 20 mL.
[0011] Preferably, the reaction temperature is 40°C.
[0012] Preferably, the reaction time is 10 h.
[0013] Preferably, the amount of the catalyst is 20 mg.
[0014] Preferably, the reaction device is a high-pressure reactor with a volume of 50 mL.
[0015] Preferably, the two-dimensional layered transition metal compound includes two-dimensional layered transition metal sulfides, oxides, carbides, nitrides, phosphides, hydroxides and hybrid structures thereof, wherein the hybrid structures include doping or loading single atoms, constructing heterojunctions and complexes; the transition metals include V, Ti, Zr, Ta, Nb, Mo, W and Re.
[0016] Another aspect of the present invention provides a method for preparing a two-dimensional layered transition metal compound, the method comprising the following steps:
[0017] (1) adding a transition metal precursor to a solvent, then mixing it with a sulfur source, sealing it in a high-pressure reactor under the protection of an inert gas, heating it to 100-600° C. at a heating rate of 0.5-40° C. / min, and maintaining it for 1-24 h to obtain an intermediate I;
[0018] (2) treating the intermediate I obtained in step (1) in an alkaline solution with stirring for 1 to 3 hours, washing, filtering and drying to obtain intermediate II;
[0019] (3) treating the intermediate II obtained in step (2) at 100 to 300° C. for 1 to 3 hours under a hydrogen atmosphere to remove impurities on the catalyst surface and introduce vacancies to obtain the two-dimensional layered transition metal sulfide;
[0020] (4) transferring the obtained two-dimensional layered transition metal sulfide into a tube furnace, introducing high-purity air, heating the temperature to 100-800° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 h to obtain a two-dimensional layered transition metal oxide;
[0021] or transferring the obtained two-dimensional layered transition metal sulfide into a tubular furnace, introducing methane gas, heating the temperature to 300-1000° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 hours to obtain a two-dimensional layered transition metal carbide;
[0022] Or the prepared two-dimensional layered transition metal sulfide is transferred into a tube furnace, sodium hypophosphite is introduced, and the temperature is raised to 200-400° C. at a heating rate of 0.5-10° C. / min in an inert atmosphere, and maintained for 1-24 hours to obtain a two-dimensional layered transition metal phosphide;
[0023] Or the prepared two-dimensional layered transition metal sulfide is mixed with an alkaline solution with a concentration of 1 to 6 mol / L, sealed in a high-pressure reactor under the protection of an inert gas, and programmed to heat to 100 to 240° C., maintained for 10 to 24 hours, to obtain a two-dimensional layered double hydroxide (LDHs).
[0024] Preferably, in step (1), the transition metal precursor is at least one of ammonium metavanadate, ammonium molybdate, tungstate, ammonium perrhenate, niobium chloride, tantalum chloride, titanium chloride, tetrabutyl titanate, zirconium oxychloride, etc.; the sulfur source is at least one of carbon disulfide, selenium powder or tellurium powder; and the molar ratio of the transition metal precursor to sulfur atoms is 1:2-1:500.
[0025] Preferably, in step (1), the solvent is at least one of water, acetone, methanol, ethanol, ammonia, ethylene glycol, N,N-dimethylformamide, toluene, acetonitrile, ethylenediamine, chloroform, formic acid and diethyl ether.
[0026] Preferably, in step (2), the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution, and the concentration of the sodium hydroxide solution or the potassium hydroxide solution is 5 to 50 wt.%; the stirring rate is 200 to 1000 rpm; the washing process is washing with ultrapure water and ethanol until the solution is neutral; the drying temperature is 25 to 150° C., and the drying time is 6 to 24 hours.
[0027] On the other hand, the present invention provides a method for preparing a two-dimensional layered transition metal compound containing a hybrid structure, wherein the two-dimensional layered transition metal compound prepared by the above preparation method is doped and loaded with metal / non-metal atoms, and transition metal compounds of different crystalline phases are stacked to obtain its hybrid structure.
[0028] Preferably, the doped or loaded metal atom is at least one of Ti, Bi, Fe, Cu, Ag, Au, Ru, Ir, Pt, and Pd; the doped or loaded non-metal atom is at least one of B, C, N, P, F, Cl, Br, or I; the doped or loaded metal atom precursor is one or more of tetrabutyl titanate, bismuth nitrate pentahydrate, iron nitrate nonahydrate, copper nitrate trihydrate, silver nitrate, chloroauric acid, palladium chloride, ruthenium chloride, ammonium chloroiridate, or chloroplatinic acid; the doped or loaded non-metal atom precursor is at least one of boric acid, CO, CO2, NH3, phosphoric acid, sodium fluoride, sodium chloride, sodium iodide, etc.; the stacking method between transition metal compounds of different crystalline phases is in-situ growth or physical compounding.
[0029] The method for preparing ethylene glycol by direct catalysis of ethylene from oxygen in one step has the following advantages over the commonly used step-by-step process in industry: (1) the shorter reaction process avoids the cost increase caused by the purification and separation process related to the intermediates; (2) the milder reaction conditions further bring significant environmental and process benefits, such as lower heat energy input, a wider range of catalyst options and safer operating conditions; (3) oxygen as an oxidant has a wide source and is economical, which can further reduce the production cost of ethylene glycol. At the same time, ethylene as a raw material can be obtained from greenhouse gas CO2 or biomass, which can achieve sustainable production of ethylene glycol.
[0030] The beneficial effects of the present invention are:
[0031] 1. The present invention is the first to use two-dimensional layered transition metal compounds and their hybrid structures in an ethylene oxidation system to directly catalyze the conversion of ethylene into ethylene glycol at room temperature or even lower temperatures.
[0032] 2. The present invention provides a universal strategy for preparing two-dimensional transition metal compounds. The prepared two-dimensional layered transition metal compounds have the advantages of uniform distribution, fewer layers, and clear structure.
[0033] 3. The present invention successfully achieves the regulation of the electronic structure and performance of two-dimensional transition metal compounds through hybridization means such as doping, loading, and construction of heterojunctions or composites. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a graph showing the activity evaluation results of the catalysts prepared in Examples 1 to 11 and Comparative Examples 1-6 for catalytic oxidation of ethylene to produce ethylene glycol. DETAILED DESCRIPTION
[0035] The present invention is further described below by way of examples, but the scope of the claims of the present invention is not limited by these examples. Meanwhile, the examples only provide partial conditions for achieving this purpose, but do not mean that these conditions must be met to achieve this purpose.
[0036] Example 1
[0037] (1) Dissolve 900 mg of ammonium molybdate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0038] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0039] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0040] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tubular furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a MoS2 catalyst.
[0041] Example 2
[0042] (1) Dissolve 900 mg of ammonium tungstate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0043] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0044] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0045] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a WS2 catalyst.
[0046] Example 3
[0047] (1) Disperse 900 mg of ammonium molybdate and 900 mg of selenium powder in 29.4 mL of water, shake thoroughly to dissolve, then add 0.6 mL of anhydrous ethanol, mix well, and seal in a 40 mL high pressure reactor;
[0048] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0049] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0050] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace and calcined at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a MoSe2 catalyst.
[0051] Example 4
[0052] (1) Disperse 900 mg of ammonium molybdate and 900 mg of tellurium powder in 29.4 mL of water, shake thoroughly to dissolve, then add 0.6 mL of anhydrous ethanol, mix well, and seal in a 40 mL high pressure reactor;
[0053] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0054] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0055] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a MoTe2 catalyst.
[0056] Example 5
[0057] (1) Dissolve 900 mg of ammonium molybdate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0058] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0059] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0060] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain MoS2;
[0061] (5) The prepared MoS2 is transferred into a tubular furnace, high-purity air is introduced, and the temperature is maintained at 500°C for 2 h with a programmed heating rate of 10°C / min to obtain a MoO3 catalyst.
[0062] The catalyst was used to catalyze the one-step oxidation of ethylene to ethylene glycol, and the activity evaluation results are listed in Figure 1 .
[0063] Example 6
[0064] (1) Dissolve 900 mg of ammonium molybdate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0065] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0066] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0067] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain MoS2;
[0068] (5) The prepared MoS2 is transferred into a tubular furnace, high-purity methane is introduced, and the temperature is maintained at 800°C for 2 h with a programmed heating rate of 10°C / min to obtain a MoC catalyst.
[0069] The catalyst was used to catalyze the one-step oxidation of ethylene to ethylene glycol, and the activity evaluation results are listed in Figure 1 .
[0070] Example 7
[0071] (1) Dissolve 900 mg of ammonium molybdate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0072] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0073] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0074] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain MoS2;
[0075] (5) The prepared MoS2 is transferred into a tubular furnace, ammonia is introduced, and the temperature is maintained at 800°C for 2 h with a programmed heating rate of 10°C / min to obtain a MoN catalyst.
[0076] Example 8
[0077] (1) Dissolve 900 mg of ammonium molybdate in 20 mL of water, shake thoroughly, and then add 10 mL of carbon disulfide and seal in a 40 mL high pressure reactor under argon protection;
[0078] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0079] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0080] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain MoS2;
[0081] (5) The prepared MoS2 is transferred into a tubular furnace, sodium hypophosphite is added (the mass ratio of MoS2 to sodium hypophosphite is 1:3), and the temperature is maintained at 300°C for 2 h. The programmed heating rate is 10°C / min, and MoP catalyst is obtained.
[0082] Example 9
[0083] (1) Dissolve 900 mg of ammonium molybdate and 43.4 mg of chloroauric acid in 20 mL of water, shake thoroughly to dissolve, and then seal the mixture with 10 mL of carbon disulfide in a 40 mL high-pressure reactor under inert gas protection;
[0084] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0085] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0086] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain an Au-MoS2 catalyst.
[0087] Example 10
[0088] (1) Dissolve 900 mg of ammonium molybdate, 52.7 mg of ammonium hexachlorometallic iridate, and 43.4 mg of chloroauric acid in 20 mL of water, shake thoroughly to dissolve, then add 10 mL of carbon disulfide and seal in a 40 mL high-pressure reactor under inert gas protection;
[0089] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0090] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0091] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tubular furnace and calcined at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain an IrAu-MoS2 catalyst.
[0092] Embodiment 11
[0093] (1) Dissolve 900 mg of ammonium molybdate and 43.4 mg of chloroauric acid in 20 mL of water, shake thoroughly to dissolve, and then seal the mixture with 10 mL of carbon disulfide in a 40 mL high-pressure reactor under inert gas protection;
[0094] (2) maintaining the high pressure reactor in (1) at 400° C. for 4 h;
[0095] (3) The sample obtained in (2) was treated in 6 mol / L potassium hydroxide solution for 3 h, and then washed with ultrapure water and ethanol respectively and filtered;
[0096] (4) The sample obtained in (3) was dried at 60°C and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain an Au-MoS2 sample.
[0097] (5) Au-MoS 2. The sample was transferred into a tube furnace, sodium hypophosphite was added (the mass ratio of Au-MoS2 to sodium hypophosphite was 1:3), and the temperature was maintained at 300°C for 2 h with a programmed heating rate of 10°C / min to obtain the Au-MoP catalyst.
[0098] Comparative Example 1
[0099] (1) Take 200 mg of commercial Al2O3 powder and dissolve it in 20 mL of water. Then, add 16.08 mg of silver nitrate and shake it thoroughly to dissolve it. Then, place the dispersion in a fume hood and stir it at room temperature and pressure until it is dry. The rotation speed is r = 500 rpm.
[0100] (2) The sample obtained in (1) was fully ground in a mortar and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a 5% Ag / Al2O3 catalyst.
[0101] Comparative Example 2
[0102] (1) Take 200 mg of commercial Al2O3 powder and dissolve it in 20 mL of water. Then, shake it thoroughly to make it evenly dispersed. Then, add 32.16 mg of silver nitrate and shake it thoroughly to dissolve it. Then, place the dispersion in a fume hood and stir it at room temperature and pressure at a speed of r = 500 rpm.
[0103] (2) The sample obtained in (1) was fully ground in a mortar and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a 10% Ag / Al2O3 catalyst.
[0104] Comparative Example 3
[0105] (1) Take 200 mg of commercial Al2O3 powder and dissolve it in 20 mL of water. Then, shake it thoroughly to make it evenly dispersed. Then, add 64.32 mg of silver nitrate and shake it thoroughly to dissolve it. Then, place the dispersion in a fume hood and stir it at room temperature and pressure at a speed of r = 500 rpm.
[0106] (2) The sample obtained in (1) was fully ground in a mortar and then transferred into a tube furnace for calcination at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a 20% Ag / Al2O3 catalyst.
[0107] Comparative Example 4
[0108] (1) 100 mg of commercial MoC sample was transferred into a tube furnace and calcined at 300 °C for 2 h in high-purity hydrogen with a programmed heating rate of 10 °C / min to obtain Bulk-MoC catalyst.
[0109] Comparative Example 5
[0110] 100 mg of commercial MoN sample was transferred into a tubular furnace and calcined at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain a Bulk-MoN catalyst.
[0111] Comparative Example 6
[0112] 100 mg of commercial MoS2 sample was transferred into a tubular furnace and calcined at 300°C for 2 h in high-purity hydrogen with a programmed heating rate of 10°C / min to obtain Bulk-MoS2 catalyst.
[0113] Application Example 1
[0114] The catalysts prepared in Examples 1 to 11 and Comparative Examples 1 to 6 were used to evaluate the activity of catalytic oxidation of ethylene to ethylene glycol. The activity evaluation results are listed in Figure 1 .
[0115] Gas production unit: Dalian Data Gas Co., Ltd.; Gas purity: 99.999%
[0116] 1. Use a 50mL high-pressure reactor and a matching thermocouple stirrer as the reaction vessel;
[0117] 2. Reaction temperature: 40°C;
[0118] 3. Reaction gas: 1bar C2H4, 1bar O2 and 10bar CO mixture;
[0119] 4. Reaction pressure: 12 bar;
[0120] 5. Reaction solvent: 20 ml ultrapure water;
[0121] 6. Reaction time: 10h;
[0122] 7. Speed: 1200rpm;
[0123] 8. Catalyst dosage: 20 mg.
[0124] The catalyst prepared by the present invention has never been reported or applied in catalytic oxidation of ethylene, and exhibits excellent performance and stability in direct catalytic conversion of ethylene to ethylene glycol, and is expected to be industrialized.
Claims
1. A method for directly catalytically converting ethylene into ethylene glycol using oxygen, characterized in that: The reaction gas is a mixture of C2H4, O2 and CO, the reaction medium is water, the reaction temperature is -10 to 100°C, the reaction pressure is 1 to 50 bar, the reaction time is 1 to 10 hours, the catalyst is at least one of a two-dimensional layered transition metal compound and a hybrid structure thereof, the catalyst dosage is 10 to 100 mg, and the reaction device is a high-pressure reactor with a volume of 50 mL; The method for preparing the two-dimensional layered transition metal compound comprises the following steps: (1) adding a transition metal precursor to a solvent, then mixing it with a sulfur source, sealing it in a high-pressure reactor under the protection of an inert gas, heating it to 100-600° C. at a heating rate of 0.5-40° C. / min, and maintaining it for 1-24 h to obtain an intermediate I; (2) treating the intermediate I obtained in step (1) in an alkaline solution with stirring for 1 to 3 hours, washing, filtering and drying to obtain intermediate II; (3) treating the intermediate II obtained in step (2) at 100-300° C. for 1-3 h under a hydrogen atmosphere to obtain a two-dimensional layered transition metal sulfide; (4) transferring the obtained two-dimensional layered transition metal sulfide into a tube furnace, introducing high-purity air, heating the temperature to 100-800° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 h to obtain a two-dimensional layered transition metal oxide; or transferring the obtained two-dimensional layered transition metal sulfide into a tubular furnace, introducing methane gas, heating the temperature to 300-1000° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 hours to obtain a two-dimensional layered transition metal carbide; Or the prepared two-dimensional layered transition metal sulfide is transferred into a tube furnace, sodium hypophosphite is introduced, and the temperature is raised to 200-400° C. at a heating rate of 0.5-10° C. / min in an inert atmosphere, and maintained for 1-24 hours to obtain a two-dimensional layered transition metal phosphide; The preparation method of the two-dimensional layered transition metal compound containing a hybrid structure is: doping and loading the two-dimensional layered transition metal compound with metal / non-metal atoms and stacking transition metal compounds of different crystal phases to obtain its hybrid structure.
2. The method according to claim 1, characterized in that The pressure of C2H4 in the reaction gas is 1-20 bar, the pressure of O2 is 0.25-3 bar, and the pressure of CO is 1-30 bar.
3. The method according to claim 1, characterized in that: The reaction medium is ultrapure water, and the amount used is 2 to 40 mL.
4. The method according to claim 1, characterized in that The two-dimensional layered transition metal compound is selected from two-dimensional layered transition metal sulfides, oxides, carbides, nitrides, phosphides and hybrid structures thereof, and the hybrid structure is selected from doping or loading single atoms, constructing heterojunctions and composites; the transition metals include V, Ti, Zr, Ta, Nb, Mo, W, and Re.
5. A method for preparing a two-dimensional layered transition metal compound, characterized in that: The method comprises the following steps: (1) adding a transition metal precursor to a solvent, then mixing it with a sulfur source, sealing it in a high-pressure reactor under the protection of an inert gas, heating it to 100-600° C. at a heating rate of 0.5-40° C. / min, and maintaining it for 1-24 h to obtain an intermediate I; (2) treating the intermediate I obtained in step (1) in an alkaline solution with stirring for 1 to 3 hours, washing, filtering and drying to obtain intermediate II; (3) treating the intermediate II obtained in step (2) at 100 to 300° C. for 1 to 3 hours under a hydrogen atmosphere to obtain the two-dimensional layered transition metal sulfide; (4) transferring the obtained two-dimensional layered transition metal sulfide into a tube furnace, introducing high-purity air, heating the temperature to 100-800° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 h to obtain a two-dimensional layered transition metal oxide; or transferring the obtained two-dimensional layered transition metal sulfide into a tubular furnace, introducing methane gas, heating the temperature to 300-1000° C. at a heating rate of 0.5-10° C. / min, and maintaining the temperature for 1-24 hours to obtain a two-dimensional layered transition metal carbide; Alternatively, the prepared two-dimensional layered transition metal sulfide is transferred into a tubular furnace, sodium hypophosphite is introduced, and the temperature is raised to 200-400° C. at a heating rate of 0.5-10° C. / min in an inert atmosphere, and maintained for 1-24 hours to obtain a two-dimensional layered transition metal phosphide.
6. The preparation method according to claim 5, characterized in that: In step (1), the transition metal precursor is at least one of ammonium metavanadate, ammonium molybdate, tungstate, ammonium perrhenate, niobium chloride, tantalum chloride, titanium chloride, tetrabutyl titanate, and zirconium oxychloride; the sulfur source is carbon disulfide; and the molar ratio of the transition metal precursor to sulfur atoms is 1:2-1:
500.
7. The preparation method according to claim 5, characterized in that: In step (1), the solvent is at least one of water, acetone, methanol, ethanol, ammonia, ethylene glycol, N,N-dimethylformamide, toluene, acetonitrile, ethylenediamine, chloroform, formic acid, and ether.
8. The preparation method according to claim 5, characterized in that: In step (2), the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution, and the concentration of the sodium hydroxide solution or the potassium hydroxide solution is 5 to 50 wt.%; the stirring rate is 200 to 1000 rpm; the washing process is washing with ultrapure water and ethanol until the solution is neutral; the drying temperature is 25 to 150° C., and the drying time is 6 to 24 hours.
9. A method for preparing a two-dimensional layered transition metal compound containing a hybrid structure, characterized in that: The two-dimensional layered transition metal compound prepared by the preparation method according to any one of claims 5 to 8 is doped and loaded with metal / non-metal atoms and transition metal compounds of different crystal phases are stacked to obtain its hybrid structure.
10. The preparation method according to claim 9, characterized in that: The doped or loaded metal atom is at least one of Ti, Bi, Fe, Cu, Ag, AuRu, Ir, Pt, and Pd; the doped or loaded non-metal atom is at least one of B, C, N, P, F, Cl, Br, or I; the doped or loaded metal atom precursor is one or more of tetrabutyl titanate, bismuth nitrate pentahydrate, iron nitrate nonahydrate, copper nitrate trihydrate, silver nitrate, chloroauric acid, palladium chloride, ruthenium chloride, ammonium chloroiridate, or chloroplatinic acid; the doped or loaded non-metal atom precursor is at least one of boric acid, CO, CO2, NH3, phosphoric acid, sodium fluoride, sodium chloride, and sodium iodide; the stacking method between transition metal compounds of different crystalline phases is in-situ growth or physical compounding.