Electrolyte for lithium battery and lithium battery
By using thiazine-based and thiazole-based compounds with cyclic structures as film-forming additives in lithium batteries, the problem of oxidation and decomposition of the electrolyte for lithium batteries at high potential is solved, a stable interface film is formed, and the battery cycle is improved. stability and longevity.
Patent Information
- Application Number
- CN202111370137.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-18
AI Technical Summary
The electrolyte used in existing lithium batteries undergoes oxidative decomposition at high potentials, resulting in rapid electrolyte consumption, erosion of electrode materials, and structural collapse, resulting in battery expansion and rapid performance attenuation, which limits the application of high-nickel ternary materials in the field of lithium batteries.
An electrolyte including a lithium salt, an electrolyte solvent and a film-forming additive is used. The electrolyte solvent is carbonate, and the film-forming additive is a compound with a cyclic structure and its derivatives, containing a thiazine group and a thiazole group. As a film-forming additive for negative electrode film formation and positive electrode complexing, it takes priority over carbonate solvents to reduce at the negative electrode, inhibits the reduction and oxidation of carbonate solvents, reduces the consumption of active lithium, and forms a stable solid electrolyte interface film to improve the cycle of the battery core. Storage stability.
It effectively inhibits the oxidative decomposition of the electrolyte, reduces metal dissolution and structural collapse of the electrode material, improves the high-temperature cycle performance and life of the battery, and extends the service life of the battery.
Smart Images

Figure CN116137348B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium batteries, and in particular to an electrolyte for lithium batteries and a lithium battery. Background Art
[0002] High-nickel ternary positive electrode materials have high specific capacity at high potentials and can significantly improve the energy density of batteries, and therefore have been widely studied in the industry.
[0003] However, the electrolyte system composed of carbonate and lithium hexafluorophosphate in the existing lithium battery is unstable at 4.5V and will undergo oxidative decomposition, resulting in rapid consumption of the electrolyte. The generated by-products will also accelerate the side reactions of the negative electrode material, the metal dissolution and structural collapse of the positive electrode material, destroy the electrode-electrolyte interface film, and increase the impedance of the positive electrode surface, ultimately leading to battery expansion and rapid performance decay; at the same time, high-nickel materials usually undergo oxygen evolution at high potentials, thereby accelerating the oxidative decomposition and gas production of the carbonate electrolyte, ultimately leading to poor battery interface stability, increased impedance and reduced battery performance, thereby limiting the application of high-nickel ternary materials in the field of lithium batteries.
[0004] Therefore, the prior art needs to be improved. Summary of the invention
[0005] The technical problem to be solved by the present application is to provide an electrolyte for a lithium battery and a lithium battery, so as to solve the technical problem in the prior art that the electrolyte for a lithium battery undergoes oxidative decomposition under high potential, resulting in rapid consumption of the electrolyte, erosion of the electrode material and structural collapse, causing battery expansion and rapid performance decay.
[0006] In order to solve the above problems, the present application is implemented through the following technical solutions:
[0007] The present application proposes an electrolyte for a lithium battery, which includes a lithium salt, an electrolyte solvent and a film-forming additive, wherein the electrolyte solvent includes a carbonate, and the film-forming additive includes M, where M is a compound having a cyclic structure and its derivatives, and the cyclic structure contains at least one of a thiazine group and a thiazolyl group.
[0008] Furthermore, in the electrolyte, the structural formula of M is as follows:
[0009]
[0010] Among them, R 1 is one of N and S;
[0011] R 2is selected from substituted or unsubstituted C1-C6 alkylene, substituted or unsubstituted C2-C6 alkenylene, substituted or unsubstituted C2-C6 alkynylene, and the substituent is selected from at least one of halogen, carbonyl, cyano, amino, carboxyl, mercapto, oxazolyl, and C1-C3 alkyl;
[0012] R 3 is H or selected from substituted or unsubstituted alkyl, alkenyl, alkynyl, aromatic and derivatives thereof, and the substituent is at least one of halogen, carbonyl, carboxyl, hydroxyl, cyano, amino and isothiocyano.
[0013] Furthermore, in the electrolyte, M is selected from at least one of 1,2,3-dithiazine, 2H-1,2,3-thiadiazine, 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid, 2-(1,2,3-dithiazine-4-yl)ethanol 1,2,3-thiadiazole-4-carboxylic acid-5-mercapto-(9CI), 1,2,3-thiadiazole-4-carboxylic acid, 2,5-dihydro-5-imino-ethyl ester, and (E)-5-(1,2,3-thiadiazole-5(2H)-ylidene)-1,3,4-oxadiazole-2(5H)-thione.
[0014] Furthermore, in the electrolyte, the mass percentage of M is 0.1% to 10%.
[0015] Furthermore, in the electrolyte, the film-forming additive also includes one or more of fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfite, and methylene methanedisulfonate.
[0016] Furthermore, in the electrolyte, the carbonate includes cyclic carbonate and linear carbonate.
[0017] Furthermore, in the electrolyte, the cyclic carbonate includes ethylene carbonate, and the linear carbonate includes at least one of diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate.
[0018] Furthermore, in the electrolyte, the lithium salt includes lithium hexafluorophosphate.
[0019] Furthermore, in the electrolyte, the lithium salt also includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide.
[0020] The present application also provides a lithium battery, which includes the electrolyte as described above.
[0021] Furthermore, the positive electrode material of the lithium battery is a high-nickel ternary positive electrode material.
[0022] Furthermore, the positive electrode material of the lithium battery is a ternary nickel-cobalt-manganese material.
[0023] Compared with the prior art, the embodiments of the present application have the following advantages:
[0024] In an embodiment of the present application, an electrolyte for a lithium battery is provided, comprising a lithium salt, an electrolyte solvent and a film-forming additive, wherein the electrolyte solvent comprises a carbonate, and the film-forming additive comprises M, wherein M is a compound having a cyclic structure and its derivatives, wherein the cyclic structure contains at least one of a thiazinyl group and a thiazolyl group, wherein the above-mentioned film-forming additive can be used as a film-forming additive for negative electrode film formation and positive electrode complexation, and when the electrolyte comprises a lithium salt and a carbonate solvent, the additive can be reduced to form a film at the negative electrode in preference to the carbonate solvent, inhibiting the reduction of the carbonate solvent, and can complex transition metal ions at the positive electrode of the battery, thereby reducing the oxidation of the carbonate solvent, reducing the consumption of active lithium, and improving the cycle storage stability of the battery cell.
[0025] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the general structural formula of the film-forming additive M provided in the embodiments of the present application. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0028] An electrolyte for a lithium battery provided in an embodiment of the present application includes a lithium salt, an electrolyte solvent and a film-forming additive, wherein the electrolyte solvent includes a carbonate, and the film-forming additive includes M, where M is a compound having a ring structure and its derivatives, and the ring structure contains at least one of a thiazine group and a thiazolyl group.
[0029] The above-mentioned film-forming additive M can be used as a film-forming additive for negative electrode film formation and positive electrode complexation. When the electrolyte includes lithium salts and carbonate solvents, the additive can be reduced to form a film at the negative electrode in preference to the carbonate solvent, inhibiting the reduction of the carbonate solvent, and can complex transition metal ions at the positive electrode of the battery, reducing the oxidation of the carbonate solvent, reducing the consumption of active lithium, and improving the cycle storage stability of the battery cell.
[0030] Among them, during the electrochemical reaction, the thiazine and thiazolyl groups in the ring structure can be reduced to generate Li 2 O. Li 2 S. Li 3N and other inorganic components with high ion conductivity make the interface impedance lower; the double bonds of the thiazine and / or thiazolyl groups in the ring structure are electrochemically polymerized to form polymers such as polyolefins, and combined with the sulfur-nitrogen cross-linked structure, the polymer chains of the polymer components are connected to form a solid electrolyte interface film (Solid Electrolyte Interface, SEI) with a cross-linked network structure containing organic and inorganic layers, and this film has outstanding elastic properties, can adapt to the volume expansion and contraction of silicon particles in the electrochemical process without breaking, can effectively prevent the side reaction between the electrolyte and the surface of the silicon negative electrode, and greatly reduce the interface impedance, improve the high-temperature cycle performance of the battery, and extend the life of the battery; therefore, the electrolyte provided by the present application solves the technical problem that the electrolyte for lithium batteries in the prior art undergoes oxidative decomposition at high potential, resulting in rapid consumption of the electrolyte, erosion of the electrode material and structural collapse, causing battery expansion and rapid performance decay.
[0031] In addition, when the positive electrode material of the battery is a high-nickel material or other material that is prone to produce strongly oxidizing metal ions under high voltage conditions, the thiazine thiazolyl compound in the present application has multiple complexing sites, which can effectively complex the tetravalent nickel ions with strong oxidizing properties in the electrolyte, and can generate low-oxidizing multi-ring structure stable organic metal chelates, thereby preventing the strong oxidizing metal ions dissolved from the positive electrode from oxidizing the electrolyte, reducing the side reaction products of the electrolyte, and also reducing the continued dissolution of metal elements in the positive electrode material and structural collapse, thereby further improving the cycle stability and life of the battery under high voltage and high temperature.
[0032] In addition, the electrolyte solvent provided in the present application includes carbonates, and the above-mentioned film-forming additive M only forms coordination complexes through strongly electronegative atoms, so it has good compatibility with the carbonate system, is miscible, and will not affect the physicochemical properties of the parent electrolyte. It can be used in different electrolyte systems and has universal applicability.
[0033] For example, when the positive electrode material is a high-nickel ternary positive electrode material, the high-nickel material will undergo oxygen evolution at a high potential higher than 4.5V, thereby accelerating the oxidation and decomposition of the carbonate electrolyte to produce gas, ultimately leading to poor battery interface stability, increased impedance, and reduced battery performance. The structure of the above-mentioned film-forming additive M has multiple complexing sites, which can effectively chelate the tetravalent nickel ions with strong oxidizing properties. The formed chelate is stable due to its cyclic structure and can be attached to the oxidation active sites on the positive electrode surface, forming a steric hindrance between the electrolyte and the electrode surface, thereby reducing the oxidation of the electrolyte by the metal dissolution of the ternary material, reducing the side reaction products of the electrolyte, and avoiding the continued dissolution of nickel metal elements and structural collapse, thereby improving the cycle stability and life of the ternary battery at high voltage and high temperature.
[0034] Specifically, see Figure 1, the general structural formula of the above-mentioned film-forming additive M is as follows:
[0035]
[0036] Among them, R 1 is one of N and S;
[0037] R 2 is selected from substituted or unsubstituted C1-C6 alkylene, substituted or unsubstituted C2-C6 alkenylene, substituted or unsubstituted C2-C6 alkynylene, and the substituent is selected from at least one of halogen, carbonyl, cyano, amino, carboxyl, mercapto, oxazolyl, and C1-C3 alkyl;
[0038] R 3 is H or selected from substituted or unsubstituted alkyl, alkenyl, alkynyl, aromatic and derivatives thereof, and the substituent is at least one of halogen, carbonyl, carboxyl, hydroxyl, cyano, amino and isothiocyano.
[0039] Among them, when R 1 When it is nitrogen, the -S-NH-N-connected structure may have more complexing sites, which can better chelate metal ions, reduce their electrochemical reaction activity, have greater steric hindrance at the positive electrode interface, and effectively reduce the contact between the electrolyte and the electrode; when R 1 When it is S, a ring structure of -SSN- is formed. This polysulfur and nitrogen structure can connect the polymer chains of the polymer components in the SEI film to form a polymer film with a cross-linked network structure. The synergistic effect of the two makes this SEI film have outstanding elastic properties.
[0040] Among them, R 2 When the carbon chain grows, the cross-linked structure may be more complex, making the interface more stable. At the same time, the steric hindrance is greater, which effectively reduces the oxidation of the electrolyte, thereby reducing the loss of active lithium and improving the cycle storage stability of the battery cell.
[0041] Among them, R 3 The presence of halogen groups in the electrolyte can reduce the lowest unoccupied orbital LUMO energy of the additive, thereby increasing its reduction potential, while the presence of olefin groups and aromatic groups can increase the content of organic matter on the SEI layer and enhance the stability of the negative electrode interface; because the carbon chain is too long, the viscosity of the additive will be high, the electrolyte will not be easily infiltrated, and the lithium ion transmission will be difficult, so R 3 The carbon chain should not be too long, for example, it should not exceed 10 carbons.
[0042] Optionally, the film-forming additive M is selected from at least one of 1,2,3-dithiazine, 2H-1,2,3-thiadiazine, 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid, 2-(1,2,3-dithiazine-4-yl)ethanol, 1,2,3-thiadiazole-4-carboxylic acid-5-mercapto-(9CI), 1,2,3-thiadiazole-4-carboxylic acid-2,5-dihydro-5-imino-ethyl ester, and (E)-5-(1,2,3-thiadiazole-5(2H)-ylidene)-1,3,4-oxadiazole-2(5H)-thione.
[0043] Among them, the structural formula of 1,2,3-dithiazine is
[0044] The structural formula of 2H-1,2,3-thiadiazine is
[0045]
[0046] The structural formula of 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid is
[0047] The structural formula of 2-(1,2,3-dithiazin-4-yl)ethanol is
[0048]
[0049] The structural formula of 1,2,3-thiadiazole-4-carboxylic acid-5-mercapto-(9CI) is
[0050] The structural formula of 1,2,3-thiadiazole-4-carboxylic acid-2,5-dihydro-5-imino-ethyl ester is The structural formula of (E)-5-(1,2,3-thiadiazole-5(2H)-ylidene)-1,3,4-oxadiazole-2(5H)-thione is
[0051]
[0052] Optionally, in the above electrolyte, the mass percentage of M is 0.1% to 10%. If the amount of the above film-forming additive M is too small, the effect is not good, and the film-forming amount may be too small to form a dense interface layer; and if the amount of additive is too large, the interface film formed will be too thick, the impedance will be too large, and the battery performance will be affected. In addition, the excess additive is only free in the electrolyte, which is not easy to play a role and will also increase the cost of the electrolyte; therefore, the mass percentage of M in the above electrolyte is controlled to be 0.1% to 10%.
[0053] Optionally, R 1When they are nitrogen and sulfur respectively, the two film-forming additives formed can also be used together. When used together, the amount of each film-forming additive is between 0.1% and 5%, and the total amount of the two does not exceed 10%.
[0054] The film-forming additive is mainly used to form a solid electrolyte interface film on the electrode surface, thereby preventing the side reactions of the electrolyte. The film-forming additive M provided in the embodiment of the present application is mainly used as a positive electrode film-forming additive. Optionally, the above-mentioned film-forming additive also includes a negative electrode film-forming additive such as fluoroethylene carbonate (FEC), with a mass percentage of 0.1% to 10%, for example, 3%, which can form a thinner but stable low-impedance SEI film at the negative electrode. The above-mentioned negative electrode film-forming additive may also include one or more of vinyl ethylene carbonate (VEC), vinyl sulfite (ES), methylene disulfonate (MMDS), etc. Among them, when the electrolyte also contains other film-forming additives such as FEC, the polymer layer formed by FEC reduction, and the -SSN- structure can make these polymer layers intertwine to form a more stable and dense interface layer with outstanding elastic properties.
[0055] The electrolyte for lithium batteries provided in the embodiments of the present application includes cyclic carbonate and at least one linear carbonate. The cyclic carbonate has a higher dielectric constant but a high viscosity, while the linear ester has a low viscosity. When the two are used together, it is beneficial to improve the overall ionic conductivity of the electrolyte; in addition, the cyclic ester can also participate in the formation of the SEI film at the negative electrode, thereby effectively preventing the side reactions of the negative electrode. Therefore, the electrolyte solvent provided in the embodiments of the present application is a carbonate system including a cyclic carbonate and at least one linear carbonate.
[0056] Optionally, in the electrolyte of the present application, the cyclic carbonate includes ethylene carbonate, and the linear carbonate includes at least one of diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate. Specifically, the cyclic carbonate is ethylene carbonate, the linear carbonate is diethyl carbonate, and the mass ratio of ethylene carbonate to diethyl carbonate is 1:1 to 2.5:1, preferably 3:7.
[0057] In the embodiments of the present application, there are many types of lithium salts available. Optionally, the lithium salt is lithium hexafluorophosphate (LiPF6) with good comprehensive performance. The concentration of lithium hexafluorophosphate in the present application is 0.1 to 1.2 mol / L, preferably, the concentration of lithium hexafluorophosphate is 1 mol / L.
[0058] The above-mentioned lithium salts can also be added with a small amount of other lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSI) or lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), which can not only form a film on the negative electrode and enhance the stability of the SEI film, but also reduce the fluorine content, so that less hydrofluoric acid is produced, which is beneficial to improve the high-temperature performance of the electrolyte.
[0059] An embodiment of the present application also provides a lithium battery, comprising the lithium battery electrolyte as described above.
[0060] In the embodiment of the present application, the electrolyte for the lithium battery includes a lithium salt, an electrolyte solvent and a film-forming additive, the electrolyte solvent includes a carbonate, and the film-forming additive includes M, where M is a compound having a cyclic structure and its derivatives, and the cyclic structure contains at least one of a thiazinyl group and a thiazolyl group. The above-mentioned film-forming additive can be used as a film-forming additive for negative electrode film formation and positive electrode complexation. When the electrolyte includes a lithium salt and a carbonate solvent, the additive can be reduced to form a film at the negative electrode in priority to the carbonate solvent, inhibiting the reduction of the carbonate solvent, and can complex transition metal ions at the positive electrode of the battery, reducing the oxidation of the carbonate solvent, reducing the consumption of active lithium, and improving the cycle storage stability of the battery cell.
[0061] Among them, in the electrolyte of lithium batteries, the thiazine thiazolyl group in the ring structure can be reduced to generate Li 2 O. Li 2 S. Li 3 N and other inorganic components with high ion conductivity make the interface impedance lower; the double bonds of the thiazine and / or thiazolyl in the ring structure are electrochemically polymerized to form polymers such as polyolefins, and combined with the sulfur-nitrogen cross-linked structure, the polymer chains of the polymer components are connected to form a solid electrolyte interface film (Solid Electrolyte Interface, SEI) with a cross-linked network structure containing organic and inorganic layers, and this film has outstanding elastic properties, can adapt to the volume expansion and contraction of silicon particles in the electrochemical process without breaking, can effectively prevent the side reaction between the electrolyte and the surface of the silicon negative electrode, and greatly reduce the interface impedance, improve the high-temperature cycle performance of the battery, and extend the life of the battery; therefore, the electrolyte provided by the present application solves the technical problem that the electrolyte for lithium batteries in the prior art undergoes oxidative decomposition at high potential, resulting in rapid consumption of the electrolyte, erosion of the electrode material and structural collapse, causing battery expansion and rapid performance decay.
[0062] Optionally, the positive electrode material of the above-mentioned lithium battery is a high-nickel positive electrode material. Since high-nickel positive electrode materials and the like are prone to produce metal ions with strong oxidizing properties under voltage environments higher than 4.5V, at this time, the thiazine thiazolyl compound in the present application can effectively complex the tetravalent nickel ions with strong oxidizing properties in the electrolyte due to its multiple complexing sites, and can generate low-oxidizing multi-ring structure stable organic metal chelates, thereby preventing the strong oxidizing metal ions dissolved from the positive electrode from oxidizing the electrolyte, reducing electrolyte side reaction products, and also reducing the continued dissolution of metal elements and structural collapse of the positive electrode material, thereby further improving the cycle stability and life of the battery at high voltage and high temperature.
[0063] Preferably, the positive electrode material of the lithium battery is a high nickel ternary material such as a ternary nickel-cobalt-manganese material, specifically LiNi 0.33 Co 0.33 Mn 0.33 O 2 (NCM111 type), LiNi 0.4 Co 0.2 Mn 0.4 O 2 (NCM424 type), LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523 type), LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622 type), LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811 type), LiNi 0.85 Co 0.075 Mn 0.075 O 2 .
[0064] Optionally, the negative electrode of the above-mentioned lithium battery can be artificial graphite, natural graphite, mesocarbon microbeads (MCMB), silicon-carbon negative electrode, etc.
[0065] The present application is described in detail below through examples.
[0066] Performance testing method:
[0067] (1) Fully charged high temperature storage test
[0068] The test battery was charged at 0.5C (400mA) with a cut-off voltage of 4.5V, and then charged at a constant voltage of 4.5V with a cut-off current of 40mA;
[0069] The fully charged batteries were then placed in a 60°C constant temperature oven for 5 days, and the thickness of the batteries before and after storage was measured with a vernier caliper, and the results were averaged.
[0070] Then calculate the battery expansion rate (%), which is calculated by subtracting the thickness before storage from the thickness after storage, and dividing the thickness difference by the thickness before storage to obtain the percentage;
[0071] (2) Nickel dissolution test
[0072] After disassembling the battery that has been tested for high temperature storage in a fully charged state, repeatedly rinse the positive and negative electrode separators and the aluminum-plastic film with 5 mL of dichloromethane, and then send the washing liquid to an inductively coupled plasma spectrometer (ICP) for testing. The testing instrument can be an inductively coupled plasma spectrometer produced by Thermo Fisher. The testing conditions are familiar to general testers, and the results are averaged;
[0073] (3) Battery high voltage cycle test
[0074] The airbag of the test battery was cut off and vacuum sealed, placed in a constant temperature box at 25°C, and cycled 200 times at 1C (800mA) current between 2.75V and 4.5V. Then the capacity retention rate (%) was calculated, which was the percentage obtained by dividing the discharge capacity at the 300th cycle by the initial discharge capacity of the first cycle.
[0075] Example 1
[0076] (1) Preparation of electrolyte
[0077] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 2.14g of 2H-1,2,3-thiadiazine, a film-forming complexing additive, was added thereto, with a mass percentage of 0.09%.
[0078] (2) Preparation of batteries
[0079] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S1.
[0080] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0081] Example 2
[0082] (1) Preparation of electrolyte
[0083] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 6g of 2H-1,2,3-thiadiazine, a film-forming additive, was added thereto, with a mass percentage of 2.5%.
[0084] (2) Preparation of batteries
[0085] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S2.
[0086] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0087] Example 3
[0088] (1) Preparation of electrolyte
[0089] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 11.8g of 2H-1,2,3-thiadiazine, a film-forming additive, was added thereto, with a mass percentage of 5%.
[0090] (2) Preparation of batteries
[0091] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S3.
[0092] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0093] Example 4
[0094] (1) Preparation of electrolyte
[0095] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 18.9g of 2H-1,2,3-thiadiazine, a film-forming additive, was added thereto, with a mass percentage of 8%.
[0096] (2) Preparation of batteries
[0097] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S4.
[0098] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0099] Example 5
[0100] (1) Preparation of electrolyte
[0101] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 29.3g of 2H-1,2,3-thiadiazine, a film-forming complexing additive, was added thereto, with a mass percentage of 11%.
[0102] (2) Preparation of batteries
[0103] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S5.
[0104] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0105] Example 6
[0106] (1) Preparation of electrolyte
[0107] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of film-forming additive fluoroethylene carbonate was added thereto, with a mass percentage of 3%; 6g of film-forming complexing additive 2H-1,2,3-thiadiazine was added, with a mass percentage of 2.5%, and 2.3g of vinyl sulfite (PS) was added, with a mass percentage of 1%.
[0108] (2) Preparation of batteries
[0109] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2(523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery with a model of SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S6.
[0110] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0111] Example 7
[0112] (1) Preparation of electrolyte
[0113] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%; and 11.8g of 2-(1,2,3-dithiazin-4-yl)ethanol, a film-forming additive, was added thereto, with a mass percentage of 5%.
[0114] (2) Preparation of batteries
[0115] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2(523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S7.
[0116] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0117] Example 8
[0118] (1) Preparation of electrolyte
[0119] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate (3% by mass) as a film-forming additive was added thereto; and 11.8g of 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid (5% by mass) as a film-forming additive was added thereto.
[0120] (2) Preparation of batteries
[0121] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2(523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S8.
[0122] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0123] Example 9
[0124] (1) Preparation of electrolyte
[0125] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1mol / L. Then 7.1g of fluoroethylene carbonate (3% by mass), a film-forming additive, was added thereto; and 11.8g of 2,5-dihydro-5-imino-ethyl ester (5% by mass), a film-forming additive, was added thereto.
[0126] (2) Preparation of batteries
[0127] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery S9.
[0128] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0129] Comparative Example 1
[0130] (1) Preparation of electrolyte
[0131] 60 g of ethylene carbonate (EC) and 140 g of diethyl carbonate (DEC) were mixed to form a mixed solvent, and 30 g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent so that the lithium salt concentration was 1 mol / L.
[0132] (2) Preparation of batteries
[0133] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery DS1.
[0134] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0135] Comparative Example 2
[0136] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1 mol / L. Then 7.1g of fluoroethylene carbonate, a film-forming additive, was added thereto, with a mass percentage of 3%.
[0137] (2) Preparation of batteries
[0138] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery DS2.
[0139] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0140] Comparative Example 3
[0141] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added into the mixed solvent to make the lithium salt concentration 1 mol / L. Then 11.8g of thiadiazine was added thereto, with a mass percentage of 5%.
[0142] (2) Preparation of batteries
[0143] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2 (523 type) ternary nickel-cobalt-manganese, 100 parts of ternary nickel-cobalt-manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery of model SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery DS3.
[0144] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0145] Comparative Example 4
[0146] 60g of ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) were mixed into a mixed solvent, and 30g of lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to make the lithium salt concentration 1 mol / L. Then 7.1g of fluoroethylene carbonate (3% by mass) as a film-forming additive was added thereto; and 11.8g of thiadiazole (5% by mass) as a film-forming additive was added thereto.
[0147] (2) Preparation of batteries
[0148] 100 parts of graphite material, 1 part of conductive agent super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) binder were mixed into a uniform paste, evenly coated on the copper foil as the negative electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain the electrode sheet. The positive electrode uses LiNi 0.5 Co 0.2 Mn 0.3 O 2(523 type) ternary nickel cobalt manganese, 100 parts of ternary nickel cobalt manganese, 2 parts of carbon nanotubes (CNT), 1 part of conductive agent super-p, and 2 parts of polyvinylidene fluoride (PVDF) were mixed into a uniform paste, evenly coated on aluminum foil as the positive electrode current collector, and dried at 80°C under vacuum for 24 hours to obtain a pole piece. The battery cell was wound to prepare a soft-pack battery with a model of SL582736. In an argon glove box with a water content of less than 5ppm, 1.6g of the above-prepared electrolyte was injected into the soft-pack battery to prepare the test battery DS4.
[0149] Formation process: The simulated battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10 hours to fully wet the battery electrode sheets; after the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10 hours to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V.
[0150] Electrolyte sample composition:
[0151] The electrolyte compositions of Examples 1 to 9 and Comparative Examples 1 to 4 are shown in Table 1.
[0152] Table 1
[0153] Electrolyte No. Solvent composition Additive composition Example 1 EC / DEC=60 / 140 0.09% 2H-1,2,3-thiadiazine + 3% FEC Example 2 EC / DEC=60 / 140 2.5% 2H-1,2,3-thiadiazine + 3% FEC Example 3 EC / DEC=60 / 140 5% 2H-1,2,3-thiadiazine + 3% FEC Example 4 EC / DEC=60 / 140 8% 2H-1,2,3-thiadiazine + 3% FEC Example 5 EC / DEC=60 / 140 11% 2H-1,2,3-thiadiazine + 3% FEC Example 6 EC / DEC=60 / 140 2.5% 2H-1,2,3-thiadiazine + 3% FEC + 1% PS Example 7 EC / DEC=60 / 140 5% 2-(1,2,3-dithiazin-4-yl)ethanol + 3% FEC Example 8 EC / DEC=60 / 140 5% 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid + 3% FEC Example 9 EC / DEC=60 / 140 5% 2,5-dihydro-5-imino-ethyl ester + 3% FEC Comparative Example 1 EC / DEC=60 / 140 none Comparative Example 2 EC / DEC=60 / 140 3% FEC Comparative Example 3 EC / DEC=60 / 140 5% Thiadiazine + 3% FEC Comparative Example 4 EC / DEC=60 / 140 5% thiadiazole + 3% FEC
[0154] Sample performance test:
[0155] The above test batteries S1-S9 and DS1-DS4 were subjected to full-charge high-temperature storage tests in sequence, and the test results are shown in Table 2 below:
[0156] Table 2
[0157] Battery ID Expansion rate (%) S1 59.1 S2 20.7 S3 21.1 S4 22.3 S5 56.2 S6 14.8 S7 20.9 S8 21.3 S9 214 DS1 88.7 DS2 80.1 DS3 23.2 DS4 22.9
[0158] The above test batteries S1-S9 and DS1-DS4 were subjected to nickel element dissolution tests in sequence, and the test results are shown in Table 3 below:
[0159] Table 3
[0160] Battery ID Nickel dissolution from positive electrode (ppm) S1 6.7 S2 2.2 S3 1.7 S4 2.0 S5 5.9 S6 1.0 S7 1.8 S8 2.1 S9 1.9 DS1 12.9 DS2 9.2 DS3 2.2 DS4 2.3
[0161] The above test batteries S1-S9 and DS1-DS4 were subjected to battery high voltage cycle tests in sequence, and the test results are shown in Table 4 below:
[0162] Table 4
[0163] Battery ID Capacity retention rate (%) S1 42.4 S2 65.7 S3 68.1 S4 67.3 S5 41.2 S6 85.4 S7 68.2 S8 67.9 S9 67.1 DS1 31.1 DS2 38.9 DS3 66.3 DS4 66.9
[0164] By comparing Examples 1 to 4 and Tables 2 to 4, it can be seen that the film-forming additive M of the present application does not affect the physicochemical properties of the parent electrolyte within the mass percentage range of 0.09% to 8%, and can significantly reduce the expansion rate of the high-nickel ternary battery during high-temperature storage at full charge, improve the safety performance of the high-nickel ternary battery at high temperature, and reduce the dissolution of metallic nickel during high-temperature storage of the battery, thereby improving the capacity retention rate of the high-nickel ternary battery during the cycle at a high voltage of 4.5V;
[0165] It can be seen from Example 1 and Example 5 that when the mass percentage of the film-forming additive M in the example reaches 11%, the improvement of the performance of the ternary battery by the film-forming additive will be deteriorated.
[0166] It can be seen from Example 2 and Example 6 that the film-forming additive M in the examples of the present application is used in combination with the film-forming additive PS to achieve better results.
[0167] To sum up, in this embodiment, the electrolyte for the lithium battery includes a lithium salt, an electrolyte solvent and a film-forming additive, the electrolyte solvent includes a carbonate, and the film-forming additive includes M, where M is a compound having a cyclic structure and its derivatives, and the cyclic structure contains a thiazine group, a thiazolyl group and a double bond, wherein the above-mentioned film-forming additive can be used as a film-forming additive for negative electrode film formation and positive electrode complexation. When the electrolyte includes a lithium salt and a carbonate solvent, the additive can be reduced to form a film at the negative electrode in priority to the carbonate solvent, inhibit the reduction of the carbonate solvent, and can complex transition metal ions at the positive electrode of the battery, reduce the oxidation of the carbonate solvent, reduce the consumption of active lithium, and improve the cycle storage stability of the battery cell.
[0168] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.
[0169] The above is a detailed introduction to an electrolyte for a lithium battery and a lithium battery provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for a person skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. An electrolyte for a lithium battery, characterized in that: It includes a lithium salt, an electrolyte solvent and a film-forming additive, wherein the electrolyte solvent includes a carbonate, and the film-forming additive includes M, wherein M is a compound having a cyclic structure and a derivative thereof, wherein the cyclic structure contains at least one of a thiazine group and a thiazolyl group; The structural formula of M is as follows: Wherein, R1 is one of N and S; R2 is selected from substituted or unsubstituted C1-C6 alkylene, substituted or unsubstituted C2-C6 alkenylene, substituted or unsubstituted C2-C6 alkynylene, and the substituent is selected from at least one of halogen, carbonyl, cyano, amino, carboxyl, thiol, oxazolyl, and C1-C3 alkyl; R3 is H or selected from substituted or unsubstituted alkyl, alkenyl, alkynyl, aromatic group and derivatives thereof, and the substituent is selected from at least one of halogen, carbonyl, carboxyl, hydroxyl, cyano, amino and isothiocyano; In the electrolyte, the mass percentage of M is 2.5% to 8%.
2. The electrolyte according to claim 1, characterized in that M is selected from at least one of 1,2,3-dithiazine, 2H-1,2,3-thiadiazine, 2,5-dihydro-1,2,3-thiadiazole-4-carboxylic acid, 2-(1,2,3-dithiazin-4-yl)ethanol, 1,2,3-thiadiazole-4-carboxylic acid-5-mercapto-(9CI), 1,2,3-thiadiazole-4-carboxylic acid-2,5-dihydro-5-imino-ethyl ester, and (E)-5-(1,2,3-thiadiazole-5(2H)-ylidene)-1,3,4-oxadiazole-2(5H)-thione.
3. The electrolyte according to claim 1, characterized in that The film-forming additive further comprises one or more of fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfite, and methylene methane disulfonate.
4. The electrolyte according to claim 1, characterized in that The carbonate includes at least one of a cyclic carbonate and a linear carbonate.
5. The electrolyte according to claim 4, characterized in that The cyclic carbonate includes ethylene carbonate, and the linear carbonate includes at least one of diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate.
6. The electrolyte according to claim 1, characterized in that The lithium salt includes lithium hexafluorophosphate.
7. The electrolyte according to claim 6, characterized in that The lithium salt further comprises at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide.
8. A lithium battery, characterized in that: Comprising the electrolyte as described in any one of claims 1 to 7.
9. The lithium battery according to claim 8, characterized in that: The positive electrode material of the lithium battery is a high-nickel positive electrode material.
10. The lithium battery according to claim 9, characterized in that: The positive electrode material of the lithium battery is a ternary nickel-cobalt-manganese material.
Citation Information
Patent Citations
Non-aqueous electrolyte, preparation method thereof and lithium ion battery
CN112701351A