Treatment method and finished product of stabilized and solidified electrolytic manganese slag
By treating electrolytic manganese slag with lightly calcined magnesium oxide and magnesium chloride, a highly active MgO-MgCl2-H2O ternary system is generated, forming a high-strength solidified body. This solves the problems of low treatment strength and low utilization rate of electrolytic manganese slag, and realizes the stable solidification and efficient recycling of electrolytic manganese slag.
Patent Information
- Application Number
- CN202310001673.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-01-03
AI Technical Summary
The existing technologies for harmless treatment of electrolytic manganese slag have low strength, narrow application range, are prone to secondary pollution, are difficult to achieve full-scale treatment, and have low utilization rate.
A combination of lightly calcined magnesium oxide, magnesium chloride, and water is used to treat electrolytic manganese slag through stirring and vibration molding, generating a highly active MgO-MgCl2-H2O ternary system. This system forms needle-like 518 and 318 phases, which physically encapsulate the electrolytic manganese slag particles, adsorb manganese ions and ammonia nitrogen, and generate substances such as NH4H(PO3)2 and MnSiO3, thus achieving stable solidification.
It achieves efficient and stable solidification of electrolytic manganese slag, with a compressive strength of over 82.62 MPa and manganese ion and ammonia nitrogen content lower than the national standard. Electrolytic manganese slag can be recycled as a green cementitious material.
Smart Images

Figure HDA0004035138760000011 
Figure HDA0004035138760000012 
Figure HDA0004035138760000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmentally friendly treatment of electrolytic manganese slag, and in particular to a treatment method and a finished product of stable and solidified electrolytic manganese slag. Background Art
[0002] Electrolytic manganese slag is a byproduct of the electrolytic manganese metal process, which is produced by acid leaching, neutralization and pressure filtration of manganese carbonate powder. Electrolytic manganese slag is a harmful industrial solid waste. At present, when 1 ton of metallic manganese is produced, about 10-12 tons of electrolytic manganese slag is produced. In the past few decades, my country's electrolytic manganese slag has exceeded 10 million tons. Electrolytic manganese slag stored in the open air occupies many plots of land and contains harmful substances such as soluble ions, which seriously damages the ecological environment. In particular, under the action of rainwater washing and leaching, the soluble Mn2+ and NH4+-N in the electrolytic manganese slag will slowly migrate into the surrounding soil and water. If the human body ingests excessive manganese and ammonia nitrogen, the metabolism and insulin in the body will be disordered, and in severe cases, it will cause cancer, deformity, liver damage, etc. Therefore, the treatment of electrolytic manganese slag is a key issue in the process of new industrialization.
[0003] At present, most of the harmless treatment agents for electrolytic manganese slag are magnesium oxide + phosphate, sodium hydroxide, quicklime, etc. Most of the research on the treatment of electrolytic manganese slag with magnesium oxide + phosphate, sodium hydroxide and quicklime has low intensity, narrow application range, low utilization rate of electrolytic manganese slag, especially in different acid and alkali environments, which is easy to cause the destruction of the solid body and secondary pollution, seriously affecting industrial application and difficult to achieve full quantitative treatment. Summary of the invention
[0004] In view of the above-mentioned defects of the prior art, the purpose of the present invention is to provide a treatment method and a finished product for stabilizing and solidifying electrolytic manganese slag, which can effectively solidify the soluble manganese ions and ammonia nitrogen in the electrolytic manganese slag. At the same time, it also has high strength and can be used as a green gelling material, which is convenient for the full quantitative recycling of electrolytic manganese slag.
[0005] The objective of the present invention is achieved through such technical solution:
[0006] The method for treating the stable and solidified electrolytic manganese slag comprises the following steps:
[0007] S1, take 350-450 parts of electrolytic manganese slag, 110-170 parts of light-burned magnesium oxide, 80-120 parts of magnesium chloride, and 130-170 parts of water in proportion by weight;
[0008] S2. Mix the electrolytic manganese slag and lightly burned magnesium oxide and pre-stir for 2 minutes, then add magnesium chloride and water and stir for 5 minutes and wait for natural solidification.
[0009] Furthermore, in step S1, the electrolytic manganese slag is 400-450 parts, the light-burned magnesium oxide is 140-170 parts, the magnesium chloride is 100-120 parts, and the water is 150-170 parts.
[0010] Furthermore, in step S1, the electrolytic manganese slag is 400 parts, the light-burned magnesium oxide is 140 parts, the magnesium chloride is 100 parts, and the water is 150 parts.
[0011] The finished product obtained by the treatment method of stabilizing and solidifying electrolytic manganese slag is that the slurry after mixing and stirring in step S2 is placed in a fixed mold for vibration molding and then cured to finally obtain the finished product.
[0012] Due to the adoption of the above technical solution, the present invention has the following advantages:
[0013] 1. The light MgO in the total amount of magnesium chloride and magnesium oxide has high activity and adsorption performance, which can effectively fix the metal manganese ions and ammonia nitrogen in the electrolytic manganese slag, so that the content of metal manganese ions and ammonia nitrogen in the solidified body leachate is lower than the national standard, achieving the purpose of harmless treatment. At the same time, the solidified body has high strength, and the electrolytic manganese slag can be recycled as a green cementitious material.
[0014] 2. Light MgO in the total amount of magnesium chloride and magnesium oxide has a high activity and can react with water to generate Mg2+ and OH-. When light MgO reacts with water to generate MgOH+ and OH-, the generated OH- reacts with divalent manganese ions (MnSO4) in electrolytic manganese slag to generate Mn(OH)2 precipitation. Mn(OH)2 is easily oxidized in the air to generate insoluble tetravalent manganese ions (MnO2). In addition, the ammonia generated by the reaction of OH- in light MgO with NH4+-N is released into the air.
[0015] 3. The needle-shaped 518 phase and 318 phase generated in the solidified body have strong physical and mechanical properties and dense structure, cross-wrapped with electrolytic manganese slag particles, and played a physical wrapping role on heavy metal ions. At the same time, it also inhibits the migration of manganese ions and ammonia nitrogen. At the same time, NH4H(PO3)2, MnSiO3, Mn(MgMn)Zn2(OH)10(H2O)2 substances generated by hydration in the solidified body can effectively adsorb manganese ions and remove ammonia nitrogen.
[0016] 4. The present invention provides a detailed description of the use of the total amount of magnesium chloride and magnesium oxide to solidify electrolytic manganese slag pollutants. It is also the first time that the total amount of magnesium chloride and magnesium oxide is used to solidify electrolytic manganese slag. Although other existing technologies have mentioned it, they have not been truly implemented, and they are only briefly mentioned without truly explaining its solidification mechanism and specific implementation method.
[0017] 5. The compressive strength of the test piece made by the present invention can reach above 82.62Mpa (optimal compressive strength embodiment), which is significantly higher than the prior art in terms of strength and utilization rate.
[0018] 6. The total amount of magnesium chloride and magnesium oxide is used to solidify the electrolytic manganese slag. Through the triple effects of chemical action, physical encapsulation and physical adsorption, high efficiency and large-capacity solidification and stabilization of the electrolytic manganese slag can be achieved.
[0019] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings of the present invention are as follows:
[0021] Figure 1 This is a graph of the compressive strength of electrolytic manganese slag solids at different ages when the MgO / MgCl2 molar ratio is 5:1 and the total dosage of magnesium chloride and magnesium oxide is different in Example 1.
[0022] Figure 2 This is a graph showing the compressive strength of the electrolytic manganese slag solidified body under different MgO / MgCl2 molar ratios when the total amount of magnesium chloride and magnesium oxide in Example 1 is 35%.
[0023] Figure 3 This is the X-ray diffraction diagram of the electrolytic manganese slag solidified body at a 3-day age under the conditions in Example 1 where the MgO / MgCl2 molar ratio is 5:1 and the total dosages of magnesium chloride and magnesium oxide are 20%, 30%, 40% and 50%, respectively.
[0024] Figure 4 The X-ray diffraction pattern of the electrolytic manganese slag solidified body at 28 days of age under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total amount of magnesium chloride and magnesium oxide added is 20%, 30%, 40% and 50% respectively in Example 1
[0025] Figure 5 This is the XRD spectrum of the electrolytic manganese slag solidified body with an age of 3 days under the conditions of 35% total magnesium chloride and magnesium oxide dosage and MgO / MgCl2 molar ratio of 2, 4, 6 and 8 respectively in Example 1.
[0026] Figure 6 This is the XRD spectrum of the electrolytic manganese slag solidified body at 28 days old under the conditions of 35% total magnesium chloride and magnesium oxide content and MgO / MgCl2 molar ratio of 2, 4, 6 and 8 respectively in Example 1.
[0027] Figure 7This is a SEM image of a 3-day-old solidified electrolytic manganese slag under the conditions in Example 1 where the MgO / MgCl2 molar ratio is 5:1 and the total dosage of magnesium chloride and magnesium oxide is 25%.
[0028] Figure 8 This is a SEM image of a 3-day-old solidified electrolytic manganese slag under the conditions in Example 1 where the MgO / MgCl2 molar ratio is 5:1 and the total dosage of magnesium chloride and magnesium oxide is 35%.
[0029] Fig. 9 This is a SEM image of a 3-day-old solidified electrolytic manganese slag under the conditions in Example 1 where the MgO / MgCl2 molar ratio is 5:1 and the total dosage of magnesium chloride and magnesium oxide is 45%.
[0030] Fig.10 This is a SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio of 5:1 and total magnesium chloride and magnesium oxide dosage of 25% in Example 1.
[0031] Fig.11 This is a SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 35% in Example 1.
[0032] Fig.12 This is a SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 45% in Example 1. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0034] Embodiment 1:
[0035] The method for treating the stable and solidified electrolytic manganese slag comprises the following steps:
[0036] S1, the original slag retrieved from the slag field, dried at 105°C to constant weight, and ground into fine particles less than 3 mm by a ball mill;
[0037] S2, taking electrolytic manganese slag, light-burned magnesium oxide, magnesium chloride and water;
[0038] The above raw materials were used in the proportions of electrolytic manganese slag, light-burned magnesium oxide, magnesium chloride and water as shown in Table 1 below, and 13 experimental groups were obtained.
[0039] Experimental Group Total dosage of magnesium chloride and magnesium oxide <![CDATA[MgO / MgCl2 molar ratio]]> Water / electrolytic manganese slag <![CDATA[Water / (MgO + MgCl2)]]> B1 20% 5:1 0.38 0.6 B2 25% 5:1 0.38 0.6 B3 30% 5:1 0.38 0.6 B4 35% 5:1 0.38 0.6 B5 40% 5:1 0.38 0.6 B6 45% 5:1 0.38 0.6 B7 50% 5:1 0.38 0.6 B8 35% 2:1 0.38 0.6 B9 35% 3:1 0.38 0.6 B10 35% 4:1 0.38 0.6 B11 35% 6:1 0.38 0.6 B12 35% 7:1 0.38 0.6 B13 35% 8:1 0.38 0.6
[0040] S3, after pre-stirring the electrolytic manganese slag and light-burned magnesium oxide for 2 minutes, add magnesium chloride and water and stir for 5 minutes.
[0041] The mixed slurry was injected into a 40mm×40mm×40mm mold and vibrated for 60 times, and then the slurry was added and vibrated for another 60 times; under natural curing conditions, the mold was demoulded after curing for 48 hours.
[0042] Figure 1 The compressive strength diagram of electrolytic manganese slag solidified bodies at different ages under the conditions of MgO / MgCl2 molar ratio of 5:1 and different total amounts of magnesium chloride and magnesium oxide. Figure 1 The columns in each group of magnesium oxide and magnesium chloride dosage indicate the age from left to right as 3 days, 7 days, 14 days and 28 days.
[0043] Depend on Figure 1 It can be seen that the total amount of magnesium chloride and magnesium oxide solidified electrolytic manganese slag and showed good compressive strength. With the increase of the total amount of magnesium chloride and magnesium oxide, the hydration reaction of the MgO-MgCl2-H2O ternary system in the electrolytic manganese slag solidified body is more complete, and a mutually supporting crystal phase structure is developed, and the compressive strength of the solidified body at each age also increases accordingly. When the total amount of magnesium chloride and magnesium oxide is 30%, 35%, 40%, 45%, and 50%, the compressive strength of the solidified body at 28 days reaches 46.5Mpa, 57.8Mpa, 65.52Mpa, 73.28Mpa, and 82.62Mpa, respectively, which are all higher than the compressive strength of 42.5 ordinary silicate. When the total amount of magnesium chloride and magnesium oxide is 35%, the 28d compressive strength increases fastest. In addition, when the amount is 50%, it has the highest compressive strength at different ages. In all groups of solid bodies with a total magnesium chloride and magnesium oxide content of 20%, since magnesium oxide and magnesium chloride are evenly dispersed in the slurry, the degree of cross-linking of the MgO-MgCl2-H2O ternary system is reduced, which limits the development of the strength phase of the total magnesium chloride and magnesium oxide content in the solid body, resulting in lower compressive strength than other solid body groups.
[0044] from Figure 1 It can be seen that the strength development of the electrolytic manganese slag solid body shows an early strength trend, and all groups of solid bodies show good compressive strength at the age of 3 days. As the solid body further hydrates, the incompletely hydrated MgO reacts with water or CO2 in a humid environment to produce Mg(OH)2 and MgCO3, resulting in a decrease in the 7d compressive strength. However, as the hydration further deepens to the 14d age, the solid body produces more 318 phases and 518 phases, and the compressive strength further increases. At the 28d age, the hydration rate of the total amount of magnesium chloride and magnesium oxide in the solid body slows down, producing less 318 phase and 518 phase. Although the compressive strength is improved, the improvement is limited.
[0045] Figure 2This is the compressive strength diagram of electrolytic manganese slag solidification under different MgO / MgCl2 molar ratios with a total magnesium chloride and magnesium oxide content of 35%. Figure 2 The columns in each group of magnesium oxide and magnesium chloride dosage indicate the age from left to right as 3 days, 7 days, 14 days and 28 days.
[0046] from Figure 2 It can be seen that the order of the influence of the MgO / MgCl2 molar ratio on the compressive strength of the solidified body is: 5:1>4:1>3:1>2:1>6:1>7:1>8:1. Since the MgO / MgCl2 molar ratio of the total amount of magnesium chloride and magnesium oxide phase 5 is 5, more strength phases can be generated in the solidified body. Therefore, when the MgO / MgCl2 molar ratio is equal to 5:1, the solidified body has the best compressive strength, and its compressive strengths at 3d, 7d, 14d, and 28d are 13.5Mpa, 17.8Mpa, 22.3Mpa, and 57.8Mpa, respectively. When the MgO / MgCl2 molar ratio is lower or higher than 5:1, the compressive strength of the solidified body will decrease. This is because there are differences in the strength phases produced by different MgO / MgCl2 molar ratios in the electrolytic manganese slag solidified body. When the curing time is 3 days, the compressive strength of the solidified bodies with different molar ratios all reached above 9.5 MPa. It can be seen that when the total dosage of magnesium chloride and magnesium oxide is 35%, certain 318 phase or 518 phase is produced in the solidified bodies with different molar ratios, and the low-dose total dosage of magnesium chloride and magnesium oxide does not inhibit the production of hydration and gelation of the MgO-MgCl2-H2O ternary system in the solidified body.
[0047] Figure 3 The X-ray diffraction diagram of the electrolytic manganese slag solidified body at 3 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total amount of magnesium chloride and magnesium oxide added is 20%, 30%, 40% and 50% respectively. Figure 3 It can be seen that with the increase of the total amount of magnesium chloride and magnesium oxide, more 318 phases are produced in the early stage of solidification hydration. At the same time, the diffraction peaks of SiO2 and CaSO4·2H2O decrease. Figure 3 It can be seen that after the electrolytic manganese slag is solidified by the total amount of magnesium chloride and magnesium oxide, the crystalline phases produced are mainly: SiO2, CaSO4·2H2O, phase 518, phase 318, NH4H(PO3)2, MnSiO3, Mg(OH)2, Mn(MgMn)Zn2(OH) 10 (H2O)2. Sorrell and Annstrong found that 518 phase and 318 phase are the main crystal phases that provide strength in magnesium cement, and the strength of 518 phase is greater than that of 318 phase.
[0048] Figure 4The X-ray diffraction diagram of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total amount of magnesium chloride and magnesium oxide added is 20%, 30%, 40% and 50% respectively. Figure 4 It can be seen that after 28 days of curing, the total amount of magnesium chloride and magnesium oxide increased, which reduced the proportion of electrolytic manganese slag in the solidified body and increased the hydration and cross-linking development of MgO and MgCl2 in the solidified body. The diffraction peak intensity of SiO2, CaSO4·2H2O, and phase 318 decreased significantly, and the diffraction peak intensity of phase 518 increased significantly. The difference in crystal phase structure explains that the compressive strength of electrolytic manganese slag solidified body with high total amount of magnesium chloride and magnesium oxide and long-term curing is much higher than that of solidified body of other groups.
[0049] Figure 5 The XRD spectrum of electrolytic manganese slag solidified body at 3 days old under the conditions of 35% total magnesium chloride and magnesium oxide content and MgO / MgCl2 molar ratio of 2, 4, 6 and 8 respectively. Figure 5 It can be seen that the crystalline phases produced after the electrolytic manganese slag solidifies are mainly: SiO2, CaSO4·2H2O, 518 phase, 318 phase, NH4Fe2F, NH4H(PO3)2, Mn(MgMn)Zn2(OH)10(H2O)2, MgCl2·6H2O, Mg(OH)2. In the early stage of hydration, when the molar ratio of MgO / MgCl2 is 2, the solidified body produces more 318 phase, when the molar ratio is 4 and 6, a large amount of 518 phase and part of 318 phase are produced, and when the molar ratio is 8, the crystalline phases are mainly 518 phase and Mg(OH)2.
[0050] Figure 6 The XRD spectrum of the electrolytic manganese slag solidified body at 28 days old under the conditions of 35% total magnesium chloride and magnesium oxide content and MgO / MgCl2 molar ratio of 2, 4, 6 and 8 respectively. Figure 6It can be seen that after the solidified body is cured for 28 days, when the MgO / MgCl2 molar ratio is 2, part of the 318 phase is transformed into the 518 phase and the diffraction peak intensity of the 518 phase is enhanced. In addition, some MgCl2·6H2O crystals are precipitated in the solidified body. The diffraction peak intensity of the 518 phase produced when the molar ratio is 4 and 6 is higher, and when the molar ratio is 8, the 518 phase is reduced, and more Mg(OH)2 is produced. Since the MgO / MgCl2 molar ratio of the total amount of magnesium chloride and magnesium oxide in the 518 phase is 5, more 518 phases can be generated when the molar ratio is greater than or equal to 5, and more 318 phases are generated when it is less than 5. Therefore, when the MgO / MgCl2 molar ratio is 6 and 8, more 518 phases are generated in the solidified body, and when the molar ratio is 2 and 4, more 318 phases are generated. In addition, when the MgO / MgCl2 molar ratio is too high or too low, MgO or MgCl2 is excessive and generates Mg(OH)2 or MgCl2·6H2O, which also reduces the compressive strength of the solidified body.
[0051] Figure 7 This is the SEM image of the electrolytic manganese slag solidified body at 3 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 25%.
[0052] Figure 8 This is the SEM image of the electrolytic manganese slag solidified body at 3 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 35%.
[0053] Fig. 9 This is the SEM image of the electrolytic manganese slag solidified body at 3 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 45%.
[0054] Fig.10 This is the SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 25%.
[0055] Fig.11 This is the SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 35%.
[0056] Fig.12 This is the SEM image of the electrolytic manganese slag solidified body at 28 days old under the conditions of MgO / MgCl2 molar ratio equal to 5:1 and the total dosage of magnesium chloride and magnesium oxide being 45%.
[0057] During the hydration process of the total amount of magnesium chloride and magnesium oxide, the common strength phases are 518 phase and 318 phase. This phase has a needle-rod structure. This structure will extend along the space gaps, grow in an interlaced manner, and overlap with each other to form a dense crystalline network. Figure 7 It can be seen that the solidified body containing 25% magnesium chloride and magnesium oxide has a large number of pores at the age of 3d, and the main forms are plate-like crystals and poor 518 phase and 318 phase crystals. Fig.10 It can be seen that after 28 days of curing, the 518 phase and 318 phase crystals have improved. It is precisely because the low total amount of magnesium chloride and magnesium oxide does not form many needle-rod structures that intersect with each other, resulting in low compressive strength of the solid body. With the increase of the total amount of magnesium chloride and magnesium oxide and the increase of curing time, the pores in the solid body at 35% and 45% total amount of magnesium chloride and magnesium oxide are filled, the loose flaky crystals are reduced, and a large number of 518 phases and 318 phases are produced. The electrolytic manganese slag particles are cross-wrapped by a large number of magnesium chloride and magnesium oxide total amount of 518 phase whiskers, forming typical needle-rod whiskers in the entire solid body and forming a network structure with interlaced overlaps. This also explains why the total amount of magnesium chloride and magnesium oxide has a good curing effect on electrolytic manganese slag at the microscopic level.
[0058] In order to further analyze the leaching amount of heavy metals in the solidified body when the total amount of magnesium chloride and magnesium oxide is 35% and the molar ratio of MgO / MgCl2 is 5:1, Table 2 shows the leaching toxicity of the electrolytic manganese slag solidified body after curing for 28 days. It can be seen from Table 2 that the heavy metals in the electrolytic manganese slag can be effectively solidified, the Mn2+ solidification rate reaches 100%, and NH4+-N is also effectively controlled. There is no phenomenon of increasing the heavy metals in the electrolytic manganese slag by adding the total amount of magnesium chloride and magnesium oxide.
[0059] Table 2 Leaching toxicity of electrolytic manganese slag solid
[0060] Pollutants Concentration (mg / L) manganese <![CDATA[1.28×10 -2 ]]> Fluoride ion 0.196 mercury <![CDATA[3.6×10 -4 ]]> arsenic <![CDATA[7.6×10 -4 ]]> selenium <![CDATA[5.02×10 -3 ]]> beryllium <![CDATA[4.4×10 -3 ]]> Fluoride ion <![CDATA[5.58×10- 2 ]]> chromium <![CDATA[5.6×10 -3 ]]> Ammonia nitrogen 9.03 nickel <![CDATA[6.51×10 -2 ]]> copper 0 Zinc 0 silver 0.257 cadmium 0 barium 0 lead 0 Hexavalent Chromium 0 Methylmercury 0 Ethyl mercury 0
[0061] Mechanism of magnesium chloride, magnesium oxide, and water stabilization / solidification of manganese ions and ammonia nitrogen in electrolytic manganese slag: (1) The light MgO in the total amount of magnesium chloride and magnesium oxide has a high activity and can react with water to generate Mg 2+ and OH - When light MgO reacts with water to form MgOH + With OH - , the generated OH - It reacts with divalent manganese ions (MnSO4) in electrolytic manganese slag to form Mn(OH)2 precipitate, which is easily oxidized in air to form insoluble tetravalent manganese ions (MnO2). The chemical reaction is shown in equations (1) to (6). In addition, the pH of light MgO is alkaline and reacts with water to form OH - , when OH - With NH4 +The ammonia produced by the reaction is released into the air, and the reaction is as shown in formula (7); (2) With the change of the total proportion and dosage of magnesium chloride and magnesium oxide, a ternary system of MgO-MgCl2-H2O is formed in the electrolytic manganese slag solidification body, generating 518 phase, 318 phase, NH4H(PO3)2, NH4Fe2F, MnSiO3, Mn(MgMn)Zn2(OH) 10 (H2O)2, the needle-shaped and rod-shaped 518 phase and 318 phase cross-wrapped with the electrolytic manganese slag particles, inhibiting the migration of manganese ions and ammonia nitrogen. In addition, the generated NH4H(PO3)2, MnSiO3, NH4Fe2F, Mn(MgMn)Zn2(OH) 10 The (H2O)2 phase can also adsorb manganese ions and ammonia nitrogen.
[0062] 5MgO + MgCl2 + 13H2O→5Mg(OH)2MgCl28H2O (Phase 5) (1) 3MgO + MgCl2 + 11H2O→3Mg(OH)2MgCl28H2O (Phase 3) (2)
[0063] MgO + H2O → Mg(OH)2 → MgOH + + OH - (3)
[0064] MnSO4 + 2OH - →Mn(OH)2 + MgSO4 (4)
[0065] Mn(OH)2 + O2→MnO2 . 2H2O↓ (5) Mn(OH)2 + O2→Mn3O4↓ + 6H2O (6)
[0066] NH4 + + OH - →NH3 ↑ + H2O (7)
[0067] The above analysis and experiments show that the formula and preparation method of this embodiment have the following advantages:
[0068] (1) When the molar ratio of MgO / MgCl2 is 5:1, the compressive strength of the electrolytic manganese slag solid body increases with the increase of the total content of magnesium chloride and magnesium oxide. When the total content of magnesium chloride and magnesium oxide is 50%, the compressive strength of 28 days reaches 82.62Mpa. When the total content of magnesium chloride and magnesium oxide is 35%, the molar ratio of MgO / MgCl2 is 5:1, which is the best ratio, and the compressive strength of the solid body reaches 57.8Mpa.
[0069] (2) XRD and SEM analysis of the electrolytic manganese slag solidified body showed that the needle-shaped 518 phase and 318 phase generated in the solidified body are the main providers of mechanical strength, and at the same time, they also inhibit the migration of manganese ions and ammonia nitrogen. In addition, NH4H(PO3)2, MnSiO3, NH4Fe2F, Mn(MgMn)Zn2(OH) generated by hydration in the solidified body 10 (H2O)2 substances can also adsorb manganese ions and ammonia nitrogen.
[0070] (3) The toxicity of electrolytic manganese slag mainly comes from manganese and ammonia nitrogen. The total amount of magnesium chloride and magnesium oxide added to the electrolytic manganese slag solidified is leached to obtain Mn. 2+ It is lower than the highest requirement of emission standards. When the total content of magnesium chloride and magnesium oxide reaches 35% and the molar ratio of MgO / MgCl2 is greater than 4, the NH4+-N leached from the solidified body meets the highest requirement of emission standards, and the electrolytic manganese slag can be recycled as a green cementitious material or road base material.
[0071] Embodiment 2:
[0072] The method for treating the stable and solidified electrolytic manganese slag comprises the following steps:
[0073] S1, the original slag retrieved from the slag field, dried at 95°C to constant weight, and ground into fine particles less than 3 mm by a ball mill;
[0074] S2, take 350 parts of electrolytic manganese slag, 110 parts of light-burned magnesium oxide, 80-120 parts of magnesium chloride, 130 parts of water, 2 parts of sawn wood, 2 parts of fly ash, 2 parts of wheat straw, and 2 parts of plant fiber in proportion by weight;
[0075] S3, after pre-stirring the electrolytic manganese slag and light-burned magnesium oxide for 2 minutes, magnesium chloride and water are added and stirred for 5 minutes, and the mixed slurry is vibrated and cured in a mold to obtain a finished product.
[0076] Embodiment 3:
[0077] The method for treating the stable and solidified electrolytic manganese slag comprises the following steps:
[0078] S1, the original slag retrieved from the slag field, dried at 115°C to constant weight, and ground into fine particles less than 3 mm by a ball mill;
[0079] S2, take 450 parts of electrolytic manganese slag, 170 parts of light-burned magnesium oxide, 120 parts of magnesium chloride, 170 parts of water, 2 parts of sawn wood, and 2 parts of fly ash in proportion by weight;
[0080] S3, after pre-stirring the electrolytic manganese slag and light-burned magnesium oxide for 2 minutes, magnesium chloride and water are added and stirred for 5 minutes, and the mixed slurry is vibrated and cured in a mold to obtain a finished product.
[0081] Embodiment 4:
[0082] The method for treating the stable and solidified electrolytic manganese slag comprises the following steps:
[0083] S1, the original slag retrieved from the slag field, dried at 105°C to constant weight, and ground into fine particles less than 3 mm by a ball mill;
[0084] S2, take 400 parts of electrolytic manganese slag, 600 parts of light-burned magnesium oxide and magnesium chloride in total (wherein the molar ratio of light-burned magnesium oxide to magnesium chloride is 5), and 130-170 parts of water in proportion by weight;
[0085] S3, after pre-stirring the electrolytic manganese slag and light-burned magnesium oxide for 2 minutes, add magnesium chloride and water and stir for 5 minutes.
[0086] The mixed slurry was injected into a 40mm×40mm×40mm mold and vibrated 60 times, and then the slurry was added and vibrated again for 60 times; under natural curing conditions, the mold was removed after curing for 48 hours; the compressive strength of the hardened specimens was tested at 3 days, 7 days, and 28 days; from the crushed specimens, the test blocks with an age of 28 days were selected, and their compressive strength was tested to reach 82.63Mpa, which is higher than the strength of 42.5 ordinary Portland cement.
[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for treating stable and solidified electrolytic manganese slag, characterized in that: The following steps are involved: S1, take 350-450 parts of electrolytic manganese slag, 110-170 parts of light-burned magnesium oxide, 80-120 parts of magnesium chloride, and 130-170 parts of water in proportion by weight; S2. Mix the electrolytic manganese slag and lightly burned magnesium oxide and pre-stir for 2 minutes, then add magnesium chloride and water and stir for 5 minutes and wait for natural solidification.
2. The method for treating stable solidified electrolytic manganese slag according to claim 1, characterized in that: In step S1, the electrolytic manganese slag is 400-450 parts, the light-burned magnesium oxide is 140-170 parts, the magnesium chloride is 100-120 parts, and the water is 150-170 parts.
3. The method for treating stable solidified electrolytic manganese slag according to claim 1, characterized in that: In step S1, the electrolytic manganese slag is 400 parts, the light-burned magnesium oxide is 140 parts, the magnesium chloride is 100 parts, and the water is 150 parts.
4. The finished product obtained by the method for treating the stable solidified electrolytic manganese slag according to any one of claims 1 to 3, characterized in that: The slurry mixed and stirred in step S2 is placed in a fixed mold, vibrated and formed, and then cured to obtain a finished product.