A method for preparing a micro-nanostructured carbon-coated ternary positive electrode material
Through the preparation method of micro-nanostructured carbon-coated ternary cathode materials, the problem of balancing cycle stability and rate performance of ternary materials in lithium-ion batteries has been solved, the mechanical properties and specific surface area of the materials have been improved, and single crystal and multi-crystalline materials have been realized. Combining the advantages of crystalline materials.
Patent Information
- Application Number
- CN202310249785.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-15
AI Technical Summary
When taking into account the cycle stability and rate performance of the existing ternary cathode materials in lithium-ion batteries, the first Coulombic efficiency and compaction density are insufficient. The specific surface area of single crystal materials is too large and the mechanical properties are weak. The polycrystalline materials have large particles and poor cycle performance. Poor performance.
The preparation method of micro-nanostructured carbon-coated ternary cathode material is used, by sintering nickel, cobalt, manganese sources and lithium sources at appropriate temperatures, combined with microwave heating and ultrasonic treatment, and then using emulsifiers and carbon sources for coating. A ternary cathode material with excellent performance was prepared through microwave heating and drying.
It achieves both the advantages of single crystal and polycrystalline materials and improves the material's cycle stability and rate performance. At the same time, the carbon coating isolates the electrolyte and enhances the material's mechanical properties and specific surface area.
Smart Images

Figure CN116143197B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery positive electrode material preparation, and in particular to a method for preparing a carbon-coated ternary positive electrode material with a micro-nano structure. Background Art
[0002] Compared with lead-acid batteries, lithium-ion batteries have higher energy density and are clean and pollution-free. They are favored by the market and gradually replace lead-acid batteries to become a new generation of large-scale batteries. Among the existing lithium-ion batteries, ternary batteries are widely used in the high-end passenger car market due to their higher energy density, better low-temperature performance, and better rate performance.
[0003] Ternary positive electrode materials include single crystal and polycrystalline. When preparing single crystal materials, the ternary precursor and the lithium source are sintered into single crystal particles at a suitable temperature to improve the material's cycle stability and rate performance, but the single crystal particles have a large specific surface area, the first efficiency is often relatively low, and the compaction density is lower than that of polycrystalline. When preparing polycrystalline materials, the ternary precursor and the lithium source are sintered into polycrystalline particles at a suitable temperature to improve the material's first coulombic efficiency and compaction density. However, polycrystalline particles are larger and have a smaller specific surface area, so the first coulombic efficiency and discharge capacity are higher, the mechanical properties are weaker, and particles are prone to breakage during the cycle.
[0004] Therefore, in the preparation process, how to balance the cycle stability, rate performance, first coulombic efficiency and compaction density is an urgent problem to be solved. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a new type of ternary cathode material, which aims to combine the advantages of single crystal ternary materials and polycrystalline ternary materials to prepare a micro-nano structured ternary cathode material. At the same time, the present invention also provides a method for preparing a lithium-ion battery using the ternary cathode material.
[0006] A method for preparing a micro-nanostructured carbon-coated ternary positive electrode material comprises the following steps:
[0007] s1. Add a nickel source, a cobalt source and a manganese source into deionized water and mix them to prepare a nickel-cobalt-manganese solution, and add a lithium source into the nickel-cobalt-manganese solution to obtain a mixed solution A;
[0008] s2. Add a carbon source to the mixed solution A, stir evenly to obtain a mixed solution B, and sinter the mixed solution B after microwave heating to obtain a primary sintered sample;
[0009] s3, subjecting the primary sintered sample prepared in step s2 to ultrasonic treatment to obtain solution C;
[0010] s4, mixing octadecene and an emulsifier and stirring them so that the emulsifier is fully emulsified to obtain a solution D;
[0011] s5. Slowly drip the solution C obtained in step s3 into the solution D obtained in step s4 to obtain solution E, and dry the solution E to obtain a micro-nanostructured carbon-coated ternary positive electrode material.
[0012] Furthermore, the preparation method is as follows.
[0013] According to the molar ratio of nickel, cobalt and manganese in the required material, a nickel source, a cobalt source and a manganese source are added to a certain amount of deionized water and mixed to obtain a nickel-cobalt-manganese solution, wherein the nickel source is one of nickel nitrate, nickel sulfate and nickel acetate, the cobalt source is one of cobalt nitrate, cobalt sulfate and cobalt acetate, the manganese source is one of manganese nitrate, manganese sulfate and manganese acetate, and the molar concentration of the nickel source, the cobalt source and the manganese source is 1-6 mol / L. Subsequently, a certain amount of lithium source is added to the prepared nickel-cobalt-manganese solution to obtain a mixed solution A, wherein the lithium source is one of lithium nitrate, lithium sulfate and lithium acetate, and the ratio of the lithium source to the nickel-cobalt-manganese salt is 1:1-1:1.5.
[0014] Then, a carbon source is added to the mixed solution A, and stirred evenly to obtain a mixed solution B, wherein the carbon source is one of activated carbon, acetylene black, Ketjen black, graphene, carbon nanotubes, carbon nanofibers, and SP. The mixed solution B is added to a microwave heater, wherein the frequency of the microwave heater is 2.0-2.5 GHz, the heating power is 180-800 W, the microwave is heated to 200-600 ° C, and the temperature is kept for 5-30 minutes. The sample prepared by microwave is placed in a tube furnace for sintering, and the heating rate is 1-10 ° C / min to 800-950 ° C, and the temperature is kept for 8-20 hours to obtain a sintered sample. A protective gas needs to be introduced during the sintering process, and the protective gas is one of oxygen, air, nitrogen or argon.
[0015] The primary sintered sample was taken out, added to 10-1000 mL of distilled water, and ultrasonically treated for 10-30 min to obtain a solution C with good dispersibility. Subsequently, 10-100 mL of octadecene was measured and added to a beaker, and 0.1-10 g of an emulsifier, i.e., an amphiphilic block copolymer, was added, and stirred for 1-10 min at 4000-12000 rpm using a high-speed homogenizer to fully emulsify the emulsifier to obtain a solution D. The emulsifier was Hypermer 2524 or Hypermer 2926.
[0016] Solution C is slowly dripped into solution D, and stirring is continued at a speed of 8000-20000 rpm until the dripping is completed to obtain solution E, and solution E is placed in a drying oven and dried at 50-200°C for 1-8h until the water is completely evaporated, finally obtaining a micro-nanostructured ternary cathode material.
[0017] The prepared ternary cathode material is mixed with sucrose in a mass ratio of 1:1-20, and magnetically stirred for 1-20 hours. The stirred solution is then centrifuged and dried in a vacuum drying oven for 5-10 hours. The dried material is mixed with PVDF and NMP, placed in a tube furnace, and kept warm at 600-800°C for 1-5 hours. The protective gas is argon gas, and a button battery is prepared. The model is CR2032, denoted as NCM@C, wherein the ratio of the dried material to PVDF and NMP is any one of 8:1:1, 9:0.5:0.5, and 9.4:0.3:0.3. For comparison, the same precursor, lithium source and sintering process are used to prepare the ternary cathode material, and then the button battery is made according to the same formula, denoted as NCM.
[0018] The present invention can make up for the shortcomings of single-crystal ternary materials having too large specific surface area and polycrystalline ternary materials having poor cycle performance and rate performance, while having the advantages of both. At the same time, the outer layer coated carbon material can effectively isolate the electrolyte from the positive electrode material, thereby improving the cycle stability of the material.
[0019] There is a slight difference in the lithium ion content of the two cathode materials, mainly because NCM@C is coated with a layer of carbon on the surface, which reduces the lithium ion content of the material. In the specific surface area test, since NCM is a single crystal material, its specific surface area is relatively large, while the micro-nanostructured cathode material can submit the particle size, thereby increasing the specific surface area of the material.
[0020] After testing, the lithium ion content of the two ternary cathode materials, carbon-coated and non-carbon-coated, is slightly different, mainly because the carbon-coated ternary cathode material has a layer of carbon on the surface, which reduces the lithium ion content of the material. In the specific surface area test, since the non-carbon-coated ternary cathode material is a single crystal material, its specific surface area is relatively large, and the micro-nanostructured cathode material can increase the particle size, thereby increasing the specific surface area of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and other features, advantages and aspects of the embodiments of the present application will become more apparent with reference to the following detailed description in conjunction with the accompanying drawings. In the accompanying drawings, the same or similar reference numerals represent the same or similar elements, wherein:
[0022] Figure 1 .Impedance comparison chart of two ternary positive electrode materials with and without carbon coating. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0024] Example
[0025] According to the molar ratio of nickel, cobalt and manganese, nickel acetate, cobalt acetate and manganese acetate are added to a certain amount of deionized water for mixing, wherein the molar concentration of nickel source, cobalt source and manganese source is 2mol / L, and lithium acetate is added to nickel cobalt manganese solution at a ratio of 1:1.0.5 between nickel, cobalt and manganese source to obtain mixed solution A. Then SP is added to mixed solution 1 and stirred evenly to obtain mixed solution B. Mixed solution B is added to a microwave heater, wherein the frequency of the heater is 2.3GHz, the heating power is 780W, and the microwave heating step is to use microwaves to heat to 500℃ and keep warm for 20 minutes. After mixing, the sample is placed in a tube furnace. The sintering temperature is 880℃, the heating rate is 5℃ / min, the insulation time is 10h, and liquid oxygen is introduced. Then 10g of the sintered sample is placed in a 2000mL beaker, 1000mL of distilled water is added, and ultrasonic treatment is performed for 20min to obtain a well-dispersed solution C. Then, 50 mL of octadecene was measured and added to a beaker, 5 g of (Hypermer2524 or Hypermer2926) emulsifier (amphiphilic block copolymer) was added, and the mixture was stirred at 8000 rpm for 3 min with a high-speed homogenizer to fully emulsify Hypermer2524 to obtain solution D. Solution C was slowly dripped into solution D, and the stirring was continued at a speed of 10000 rpm until the addition was completed to obtain solution E, and solution E was placed in a drying oven at 90 ° C for 6 hours until the water was completely volatilized to obtain a micro-nanostructured ternary cathode material. Then, it was mixed with sucrose at a mass ratio of 1:5, magnetically stirred for 2 hours, and the stirred solution was centrifuged and dried in a vacuum drying oven for 8 hours, then placed in a tubular furnace, and kept warm at 700 ° C for 2 hours. The protective gas argon gas mixed the obtained ternary cathode material with PVDF and NMP in a ratio of 9.4:0.3:0.3 to prepare a button battery, model CR2032.
[0026] The present invention can make up for the shortcomings of single crystals having too large specific surface area and poor cycle performance and rate performance, while having the advantages of both. At the same time, the outer coated carbon material can effectively isolate the electrolyte from the positive electrode material, thereby improving the cycle stability of the material.
[0027] There is a slight difference in the lithium ion content of the two positive electrode materials, mainly because NCM@C is coated with a layer of carbon on the surface, which reduces the lithium ion content of the material. In the specific surface area test, since NCM is a single crystal material, its specific surface area is relatively large, and the micro-nanostructured positive electrode material can submit the particle size, thereby increasing the specific surface area of the material. The D50 of the two materials also verifies this statement. The D50 of NCM is 3.25μm, while the D50 of NCM@C is 5.71μm. Since NCM@C undergoes secondary sintering when coated with carbon, the soluble lithium of the material is lower than that of NCM.
[0028] Table 1 Comparison of physical properties of two materials
[0029]
[0030]
[0031] Figure 1 The impedance spectra of the two materials show that NCM@C has a smaller semicircle diameter and a smaller straight line slope, indicating that the charge transfer impedance and lithium ion diffusion impedance of NCM@C are smaller than those of NCM, proving that the conductivity of NCM@C is better than that of NCM.
[0032] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a micro-nanostructured carbon-coated ternary positive electrode material, characterized in that: The following steps are involved: s1. Add a nickel source, a cobalt source and a manganese source into deionized water and mix them to prepare a nickel-cobalt-manganese solution, and add a lithium source into the nickel-cobalt-manganese solution to obtain a mixed solution A; s2. Add a carbon source to the mixed solution A, stir evenly to obtain a mixed solution B, and sinter the mixed solution B after microwave heating to obtain a primary sintered sample; the microwave heating temperature is 200-600° C., and the insulation time is 5-30 min; the sintering temperature is 800-950° C., and the insulation time is 8-20 h; s3, subjecting the primary sintered sample prepared in step s2 to ultrasonic treatment to obtain solution C; s4, mixing octadecene and an emulsifier and stirring them so that the emulsifier is fully emulsified to obtain a solution D; s5. Slowly dripping the solution C obtained in step s3 into the solution D obtained in step s4 to obtain a solution E, and drying the solution E to obtain a micro-nanostructured carbon-coated ternary positive electrode material; In which, in step s2, any one of activated carbon, acetylene black, Ketjen black, graphene, carbon nanotubes, and carbon nanofibers is used as the carbon source; in step s4, the emulsifier is Hypermer 2524.
2. The preparation method according to claim 1, characterized in that: In step s1, the nickel source, cobalt source, manganese source and lithium source are all metal nitrates, sulfates or acetates.
3. The preparation method according to claim 1, characterized in that: In step s1, the ratio of the lithium source to the solute in the nickel-cobalt-manganese solution is 1:1-1:1.
5.
4. The preparation method according to claim 1, characterized in that: The amount of emulsifier added in step s4 is 0.1-10g.
5. The preparation method according to claim 1, characterized in that: In step s5, the drying temperature is 50-200° C. and the drying time is 1-8 hours.
6. Use of the micro-nanostructured carbon-coated ternary positive electrode material obtained by the preparation method according to any one of claims 1 to 5 as a positive electrode for a lithium-ion battery.