Composition for preparing ultra-thin glass, ultra-thin glass and preparation method and application thereof

By using specific compositions and processes, ultra-thin glass with excellent flexibility and bending resistance is prepared, which solves the problem of insufficient flexibility and bending resistance of UTG glass and is suitable for display devices in folding screen mobile phones.

CN116143400BActive Publication Date: 2024-10-22HEBEI GUANGXING SEMICON TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211485774.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-10-22
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

Existing UTG glass has deficiencies in flexibility and bending resistance, making it difficult to meet the stringent requirements of folding screen mobile phones.

Method used

A composition containing silica, aluminum oxide, sodium oxide, potassium oxide, barium oxide, zinc oxide, magnesium oxide and calcium oxide is used to prepare ultra-thin glass through a specific melting treatment and chemical strengthening process to improve its Flexibility and bending resistance.

Benefits of technology

The prepared ultra-thin glass has excellent flexibility and bending resistance, and is suitable as a support material for curved or folded display devices. The transmittance is as high as 92%, the Young's modulus is low, and the ultimate bending radius is small.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of ultrathin flexible glass technology, and discloses a composition for preparing ultrathin glass, the ultrathin glass itself, a method for preparing the same, and its applications. The composition contains the following components, stored individually or in combination: silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, barium oxide, zinc oxide, magnesium oxide, calcium oxide, and strontium oxide. Using the composition provided by this invention, ultrathin glass with excellent flexibility and bending resistance can be prepared, and this ultrathin glass is ideally suited for use as a support material for curved or foldable display devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultra-thin flexible glass, and in particular to a composition for preparing ultra-thin glass, ultra-thin glass and a preparation method and application thereof. Background Art

[0002] With the development of display technology, terminal display devices are no longer limited to the characteristics of flat rigid displays, but have developed displays that can be bent, rolled, and even folded. In particular, the continuous advancement of OLED display technology has made flexible displays possible.

[0003] Flexible display refers to a deformable and bendable display device made of soft materials. The current mainstream is flexible OLED technology, a fully solid-state thin film structure. In addition, flexible liquid crystal display (LCD) is also developing simultaneously, but the cost performance is relatively low.

[0004] As a new display technology, OLED (organic light emitting diode) is a self-luminous display device that uses organic thin film as the light source. Flexible OLED replaces ordinary OLED glass substrate with materials with good flexibility and good light transmittance. Its structure and light-emitting principle are similar to those of OLED devices with ordinary glass substrates.

[0005] Simply making the display screen flexible is not enough for folding phones. The screen cover also needs to be flexible. Commonly used cover glass cannot be bent freely and cannot be used as a folding cover. As a flexible cover, it must ensure flexible bending performance while taking into account strength and light transmittance, and at the same time have a certain rigidity to support the entire display component. Currently, this support method is achieved in two ways:

[0006] 1. Improve PI materials

[0007] In order to fully realize flexible display, the display cover should be able to be repeatedly bent, transparent, ultra-thin, and hard enough. Compared with the hard and fragile glass material, PI is currently the main choice. However, unlike the substrate, PI as a cover must be colorless and transparent, and PI itself is light yellow, so colorless and transparent PI becomes the key to development.

[0008] It is difficult to make colorless and transparent polyimide film, mainly because the transparency of PI film is contradictory to its high temperature resistance, that is, when the transparency of the film is to be guaranteed, its high temperature resistance will be affected. Some manufacturers have also tried to mix multiple organic materials, such as mixing PI, PMMA, PET and PU to make flexible cover plates, but the effect is not ideal and it is difficult to mass produce.

[0009] 2. Ultra-thin glass (UTG)

[0010] Glass with a thickness of less than 100 microns is usually called ultra-thin glass, which is used in the display screen of foldable consumer electronic products. UTG has two major advantages: 1. High-quality texture of glass; 2. Helps to reduce creases. As the interactive interface of flexible display terminals, flexible cover plates must not only provide necessary protection for display terminals, but also have high visible light transmittance, comfortable feel, high surface hardness, strong bending resistance and other characteristics.

[0011] Compared with PI, UTG is stronger in durability, light transmittance, hardness and texture. Chemical strengthening process can enhance the flexibility and durability of 30μm (1μm=1 / 1000000m) ultra-thin glass, and has a smooth feel and good uniformity. Considering the flexibility and surface wear resistance of the material, UTG ultra-thin inorganic glass material is expected to become the mainstream choice.

[0012] UTG has a wide range of applications, but only a small part of it can be used on foldable screen phones because foldable screens have more stringent requirements on the bendability and durability of glass. The ultra-thin glass used for foldable screen phones must not only be less than 50 microns (0.05 mm) in thickness, but also be processed and strengthened to further improve its durability.

[0013] At present, there are two major difficulties in the UTG ultra-thin flexible glass industry chain: one is the manufacturing and production of UTG ultra-thin glass as raw materials, and the other is that UTG glass must meet the required indicators for flexible cover plates, and post-processing technology must be explored.

[0014] Therefore, developing a UTG glass with good flexibility and excellent bending resistance is of great significance for the application field of folding screen mobile phones. Summary of the invention

[0015] The purpose of the present invention is to overcome the defects of UTG glass in the prior art, such as poor flexibility and poor bending resistance.

[0016] In order to achieve the above object, the first aspect of the present invention provides a composition for preparing ultra-thin glass, wherein the composition contains the following components which are stored separately or in a mixture of two or more thereof:

[0017] Silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, barium oxide, zinc oxide, magnesium oxide, calcium oxide, and strontium oxide;

[0018] Based on the total weight of the composition, the content of silicon dioxide is 55-75% by weight, the content of aluminum oxide is 1-15% by weight, the content of sodium oxide is 8-15% by weight, the content of potassium oxide is 0.1-5% by weight, the content of barium oxide is 2-10% by weight, the content of zinc oxide is 0-2% by weight, the content of magnesium oxide is 0-5% by weight, the content of calcium oxide is 0-2% by weight, and the content of strontium oxide is 0-5% by weight;

[0019] Define K1 = (Na 2 Weight percentage of O+K 2 O weight percentage) / (Al 2 O 3 The weight percentage of BaO is 20%, and K1 is not greater than 2;

[0020] Define K2=(weight percentage of MgO+weight percentage of CaO+weight percentage of SrO) / weight percentage of BaO, and K2 is 0.5-1.2;

[0021] Definition K3 = (weight percentage of MgO + weight percentage of CaO + weight percentage of SrO + weight percentage of BaO + weight percentage of ZnO) / (weight percentage of Na 2 Weight percentage of O+K 2 O weight percentage), and K3 is not less than 0.6.

[0022] Preferably, based on the total weight of the composition, the content of silicon dioxide is 57-72 weight%, the content of aluminum oxide is 3-14 weight%, the content of sodium oxide is 10-15 weight%, the content of potassium oxide is 1-3 weight%, the content of barium oxide is 2-6 weight%, the content of zinc oxide is 0.5-2 weight%, the content of magnesium oxide is 0-4 weight%, the content of calcium oxide is 0-1 weight%, and the content of strontium oxide is 0-3 weight%.

[0023] Preferably, based on the total weight of the composition, the content of silicon dioxide is 60-72 weight%, the content of aluminum oxide is 3-12 weight%, the content of sodium oxide is 12-13.5 weight%, the content of potassium oxide is 1-3 weight%, the content of barium oxide is 4-6 weight%, the content of zinc oxide is 0.5-1 weight%, the content of magnesium oxide is 0-4 weight%, the content of calcium oxide is 0-1 weight%, and the content of strontium oxide is 0-3 weight%.

[0024] Preferably, K1 is 1-1.5.

[0025] Preferably, K2 is 0.5-1.

[0026] Preferably, K3 is 0.6-1.

[0027] A second aspect of the present invention provides a method for preparing ultra-thin glass, the method comprising:

[0028] (1) contacting and mixing the components in the composition of the first aspect to obtain a mixture;

[0029] (2) subjecting the mixed material to melt treatment I and melt treatment II in sequence to obtain a molten material; wherein the temperature of the melt treatment I is lower than the temperature of the melt treatment II;

[0030] (3) The molten material is sequentially molded, annealed, thinned and chemically strengthened.

[0031] Preferably, in step (2), the temperature of the melt treatment I is 50-100°C lower than the temperature of the melt treatment II, preferably 60-80°C.

[0032] Preferably, in step (2), the conditions of the melt treatment I include at least: a temperature of 1550-1580°C and a time of 3-5h.

[0033] Preferably, in step (2), the conditions of the melt treatment II include at least: a temperature of 1600-1650° C. and a time of 4-6 h.

[0034] The third aspect of the present invention provides ultra-thin glass prepared by the method described in the second aspect.

[0035] A fourth aspect of the present invention provides use of the ultra-thin glass described in the third aspect in preparing a flexible cover plate.

[0036] The inventors of the present invention found during the research process that the composition provided by the present invention can be used to prepare ultra-thin glass with excellent flexibility and bending resistance, and the ultra-thin glass is very suitable for use as a supporting material for curved or folding display devices.

[0037] In particular, the ultra-thin glass prepared by using the composition provided by the present invention has a small Young's modulus and a small bending radius, and the transmittance of the ultra-thin glass at 550nm can reach 92%. DETAILED DESCRIPTION

[0038] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0039] It should be noted that, in various aspects of the present invention, for the same components in various aspects, the present invention is described only once in one aspect without repeated description, which should not be understood by those skilled in the art as a limitation of the present invention.

[0040] In the present invention, unless otherwise specified, the room temperature or normal temperature refers to 25±2°C.

[0041] As mentioned above, the first aspect of the present invention provides a composition for preparing ultra-thin glass, wherein the composition contains the following components which are stored independently or in a mixture of two or more thereof:

[0042] Silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, barium oxide, zinc oxide, magnesium oxide, calcium oxide, and strontium oxide;

[0043] Based on the total weight of the composition, the content of silicon dioxide is 55-75% by weight, the content of aluminum oxide is 1-15% by weight, the content of sodium oxide is 8-15% by weight, the content of potassium oxide is 0.1-5% by weight, the content of barium oxide is 2-10% by weight, the content of zinc oxide is 0-2% by weight, the content of magnesium oxide is 0-5% by weight, the content of calcium oxide is 0-2% by weight, and the content of strontium oxide is 0-5% by weight;

[0044] Define K1 = (Na 2 Weight percentage of O+K 2 O weight percentage) / (Al 2 O 3 The weight percentage of BaO is 20%, and K1 is not greater than 2;

[0045] Define K2=(weight percentage of MgO+weight percentage of CaO+weight percentage of SrO) / weight percentage of BaO, and K2 is 0.5-1.2;

[0046] Definition K3 = (weight percentage of MgO + weight percentage of CaO + weight percentage of SrO + weight percentage of BaO + weight percentage of ZnO) / (weight percentage of Na 2 Weight percentage of O+K 2O weight percentage), and K3 is not less than 0.6.

[0047] The inventors found during the research process that the composition within the aforementioned ratio range can be used to prepare ultra-thin glass with excellent flexibility and strong bending resistance, and the glass is particularly suitable for cover glass for flexible displays.

[0048] Preferably, based on the total weight of the composition, the content of silicon dioxide is 57-72 weight%, the content of aluminum oxide is 3-14 weight%, the content of sodium oxide is 10-15 weight%, the content of potassium oxide is 1-3 weight%, the content of barium oxide is 2-6 weight%, the content of zinc oxide is 0.5-2 weight%, the content of magnesium oxide is 0-4 weight%, the content of calcium oxide is 0-1 weight%, and the content of strontium oxide is 0-3 weight%.

[0049] Preferably, based on the total weight of the composition, the content of silicon dioxide is 60-72 weight%, the content of aluminum oxide is 3-12 weight%, the content of sodium oxide is 12-13.5 weight%, the content of potassium oxide is 1-3 weight%, the content of barium oxide is 4-6 weight%, the content of zinc oxide is 0.5-1 weight%, the content of magnesium oxide is 0-4 weight%, the content of calcium oxide is 0-1 weight%, and the content of strontium oxide is 0-3 weight%.

[0050] Preferably, K1 is 1-1.5. The inventors found in the research process that by adopting the specific implementation in this preferred case, a glass product with better flexibility and bending resistance can be prepared.

[0051] Preferably, K2 is 0.5-1. The inventors have found that by adopting the specific implementation of this preferred case, a glass product with better flexibility and bending resistance can be prepared.

[0052] Preferably, K3 is 0.6-1. The inventors have found that by adopting the specific implementation of this preferred case, a glass product with better flexibility and bending resistance can be prepared.

[0053] In the present invention, SiO 2 It is the main network former of glass and enables stable glass to be obtained. 2 The content will greatly increase the difficulty of glass melting and make it difficult to ensure the crystallization during the glass forming process. At the same time, too low SiO 2 The inventors found that the glass with good strength properties cannot be obtained even with a low content of SiO 2The weight percentage content is controlled at 55-75%, and combined with the other technical features of the technical solution provided by the present invention, the prepared glass has better anti-bending performance.

[0054] In the present invention, aluminum oxide is also an important factor in forming a glass network. At the same time, during the ion exchange in the chemical tempering process, aluminum oxide can promote the diffusion of alkali metal ions. Therefore, aluminum oxide can improve the ion exchangeability of glass, thereby producing high damage resistance through chemical tempering; too high aluminum oxide content makes the glass easy to crystallize and significantly increases the Young's modulus of the glass, reducing the flexibility of the glass. In addition, the inventors found that by controlling the weight percentage of aluminum oxide in the composition to 1-15%, combined with the other technical features of the technical solution provided by the present invention, a glass with a low Young's modulus and a small limit bending radius can be prepared.

[0055] In the present invention, sodium oxide belongs to alkali metal oxides, which is a glass network external oxide, can significantly reduce the viscosity of the base glass, promote the melting and clarification of the base glass, and reduce the glass crystallization temperature. At the same time, during the ion exchange in the chemical tempering process, it can be used as the object to be exchanged, for example, potassium ions with a large radius are used to replace sodium ions with a small radius, so that the ion exchange layer produces compressive stress, thereby reducing the surface micro-defects of the glass product and improving the strength of the glass product. However, the inventors found that by controlling the weight percentage of sodium oxide in the composition to 12-13.5%, combined with the other technical features of the technical solution provided by the present invention, a glass with a low Young's modulus and a small ultimate bending radius can be prepared.

[0056] In the present invention, the composition also contains potassium oxide, barium oxide, and zinc oxide. These elements have large ion radius and belong to the network outside the glass structure. The appropriate content can improve the flexibility of the glass and the anti-crystallization performance of the glass. However, too much K2O, BaO and ZnO will seriously reduce the strength performance of the glass. However, the inventors found that the weight percentage content of potassium oxide, the weight percentage content of barium oxide, and the weight percentage content of zinc oxide in the composition are controlled at 1-3%, 4-6%, and 0.5-1%, respectively, and the remaining technical features of the technical solution provided by the present invention are combined. The ultra-thin glass prepared can improve the Young's modulus and the ultimate bending radius under the premise of ensuring strength.

[0057] As mentioned above, the second aspect of the present invention provides a method for preparing ultra-thin glass, the method comprising:

[0058] (1) contacting and mixing the components in the composition of the first aspect to obtain a mixture;

[0059] (2) subjecting the mixed material to melt treatment I and melt treatment II in sequence to obtain a molten material; wherein the temperature of the melt treatment I is lower than the temperature of the melt treatment II;

[0060] (3) The molten material is sequentially molded, annealed, thinned and chemically strengthened.

[0061] The present invention has no particular limitation on the specific manner of mixing. Those skilled in the art can select technical means known in the art as needed, as long as the components can be mixed evenly to meet production requirements. The present invention exemplarily provides a preferred specific implementation method. Exemplarily, the components in the composition are introduced into a mixer for stirring and mixing.

[0062] Preferably, in step (2), the temperature of the melting treatment I is 50-100° C. lower than the temperature of the melting treatment II, more preferably 60-80° C. The inventors found in the research process that the ultra-thin glass product prepared by adopting the specific implementation of this preferred case has a lower Young's modulus and a smaller ultimate bending radius.

[0063] Preferably, in step (2), the conditions of the melt treatment I include at least: a temperature of 1550-1580°C and a time of 3-5h.

[0064] Preferably, in step (2), the conditions of the melt treatment II include at least: a temperature of 1600-1650° C. and a time of 4-6 h.

[0065] Preferably, in step (3), the forming method is flat glass product forming.

[0066] According to a preferred embodiment of the present invention, in step (3), the glass is a flat glass product, and the forming method is selected from at least one of overflow down-draw method, float method and slot down-draw method.

[0067] Preferably, in step (3), the annealing conditions at least meet the following conditions: the annealing temperature is 560-580°C.

[0068] According to a particularly preferred embodiment of the present invention, in step (3), the annealing operation comprises: forming the glass to obtain a glass ingot, placing the glass ingot into an annealing furnace set with an annealing temperature, and after the glass ingot reaches the annealing temperature, keeping the temperature for 2-3 hours, then cooling the temperature to 250°C at a cooling rate of 1°C / min, and then naturally cooling the temperature to below 50°C along with the furnace.

[0069] The method of the present invention may also include various conventional post-processing methods in the art, such as slicing, grinding, polishing, thinning, cutting and chemically strengthening the annealed product to obtain the glass. The present invention will not be described in detail here, and those skilled in the art should not be construed as limiting the present invention.

[0070] According to a preferred specific implementation manner, in step (3), the cutting method is to use a laser cutting machine to cut the glass sheets into (150-160) mm×(60-80) mm pieces.

[0071] According to a particularly preferred embodiment of the present invention, in step (3), the chemical strengthening operation comprises: placing the glass sheet obtained by cutting with a cutting machine in a potassium nitrate salt bath at 390-420° C. for treatment for 10-30 min.

[0072] As mentioned above, the third aspect of the present invention provides ultra-thin glass prepared by the method described in the second aspect.

[0073] Preferably, the ion exchange depth DOL of the ultra-thin glass is not less than 7 um, the surface compressive stress CS is not less than 400 MPa, the ultimate bending radius is not greater than 1 mm, and the Young's modulus is not greater than 70 GPa.

[0074] Preferably, the transmittance of the ultra-thin glass at a visible light wavelength of 550 nm is not less than 92%.

[0075] As mentioned above, the fourth aspect of the present invention provides the use of the ultra-thin glass described in the third aspect in the preparation of a flexible cover plate.

[0076] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all the raw materials used are commercially available products.

[0077] According to the method specified in GB / T 2680-2001, the visible light transmittance was tested using a Shimadzu UV-1900i ultraviolet-visible spectrophotometer.

[0078] The Young's modulus of glass was tested according to the method specified in GB / T 7962.6-2010.

[0079] According to the GB / T 38686-2020 method, a two-point bending tester (model WH-1408, purchased from Beijing Wohua Huitong Company) was used to test the limit bending radius of the glass.

[0080] Unless otherwise specified, the amounts of the components in the formulations in the following examples are expressed in weight percentage. 2 Taking the weight percentage as an example, the calculation method is: SiO2 Weight percentage = (SiO 2 The weight of the components in Example 1) / (the sum of the weights of the components in Example 1)×100%.

[0081] Example 1

[0082] The formula of the composition for preparing ultra-thin glass shown in Table 1 was designed, and the sum of the weights of the components in the composition was determined to be 1000 g for testing, and the masses of the corresponding components were calculated according to the formula of the composition and accurately weighed (accurate to two decimal places).

[0083] The weighed components were placed in a mixer, stirred and mixed at 20 rpm for 15 min to obtain a mixture, the mixture was poured into a platinum-rhodium crucible, placed in a high-temperature electric furnace, and heated at 1580°C for 4 h to perform melting treatment I to obtain glass liquid, and the glass liquid was heated at 1650°C for 5 h to perform melting treatment II to obtain a molten material, and then the molten material was poured into a fully preheated metal mold to cool and shape, and then the shaped glass ingot was fully annealed (specifically, the glass ingot was placed in a preheated metal mold with an annealing temperature set at 565°C). In an annealing furnace, after the glass ingot reaches the annealing temperature, it is kept warm for 2.5 hours, then cooled to 250°C at a cooling rate of 1°C / min, heating is stopped, and the temperature is naturally cooled to below 50°C with the furnace to eliminate its residual stress, and then naturally cooled to room temperature to obtain a glass ingot, and then the glass ingot is sliced, ground, polished, and thinned to form a glass sheet with a thickness of 30 microns. After the glass sheet is cleaned, it is cut into 160mm×70mm glass sheets using a laser cutting machine, and placed in a pure potassium nitrate salt bath at 410°C for treatment for 20 minutes to obtain the ultra-thin glass.

[0084] The methods of Comparative Examples 1-6 and Examples 1-6 and the total weight of the components in the composition are the same, but the weight percentage of the components in the composition is adjusted, as shown in Table 2 for details.

[0085] Table 1

[0086] Composition / weight% Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Silicon dioxide 70.00 71.50 71.50 70.5 75 57 Aluminum oxide 5.20 4.50 5.50 5.5 5 15 Sodium oxide 13.00 13.20 13.00 8 6 14 Potassium Oxide 1.00 1.00 1.00 4 1.5 0.5 Barium Oxide 6.00 5.00 4.00 8 5 6.5 Zinc Oxide 0.80 0.80 1.00 / 2 2 Magnesium Oxide 4.00 / 4.00 4 1 5 Calcium Oxide / 1.00 / / 2 / Strontium oxide / 3.00 / / 2.5 / K1 1.25 1.49 1.47 0.89 0.75 0.67 K2 0.67 0.80 1.00 0.5 1.1 0.77 K3 0.77 0.69 0.64 1 1.67 0.93 Ion exchange depth DOL / μm 14 13 15 11 8 9 Surface compressive stress / MPa 115 112 108 102 105 115 Young's modulus / GPa 66.8 67.2 67.5 68.5 68.4 69.3 Transmittance (550nm, %) 92 92 92 92 92 92 Limit bending radius / mm 0.8 0.9 0.9 1.1 1.2 1.4

[0087] Table 2

[0088] Composition / weight% Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Silicon dioxide 70.80 71.20 68.00 73.5 76 50 Aluminum oxide 4.00 8.00 10.20 2 0.5 20 Sodium oxide 13.60 14.00 14.00 8 6 16 Potassium Oxide 0.60 1.00 / 3.5 6 0.05 Barium Oxide 0.50 4.00 4.80 2 1 1 Zinc Oxide / 0.80 / / 3 3 Magnesium Oxide 4.50 / 3.00 5 0 6 Calcium Oxide 6.00 / / 1 3 3 Strontium oxide / 1.00 / 5 4.5 0.95 K1 3.16 1.25 0.93 2.88 8 0.76 K2 21 0.25 0.63 5.5 7.5 9.95 K3 0.77 0.39 0.56 1.13 0.96 0.87 Ion exchange depth DOL / μm 5 6 7 5 5 7 Surface compressive stress / MPa 80 84 86 78 75 81 Young's modulus / GPa 73.4 71.5 72.0 71 72.4 74.7 Transmittance (550nm, %) 92 92 92 92 92 92 Limit bending radius / mm 1.5 1.3 1.3 1.6 1.8 1.8

[0089] It can be seen from the above results that the ultra-thin glass prepared by the technical solution provided by the present invention has a lower Young's modulus and a smaller ultimate bending radius, and the visible light transmittance at 550nm is as high as 92%; therefore, the ultra-thin glass provided by the present invention has better flexibility and bending resistance.

[0090] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A composition for preparing ultra-thin glass, characterized in that: The composition contains the following components which are stored independently or in combination: Silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, barium oxide, zinc oxide, magnesium oxide, calcium oxide, and strontium oxide; Based on the total weight of the composition, the content of silicon dioxide is 60-72 weight%, the content of aluminum oxide is 3-12 weight%, the content of sodium oxide is 12-13.5 weight%, the content of potassium oxide is 1-3 weight%, the content of barium oxide is 4-6 weight%, the content of zinc oxide is 0.5-1 weight%, the content of magnesium oxide is 0-4 weight%, the content of calcium oxide is 0-1 weight%, and the content of strontium oxide is 0-3 weight%; Define K1=(weight percentage of Na2O+weight percentage of K2O) / (weight percentage of Al2O3+weight percentage of BaO), and K1 is 1-1.5; Define K2=(weight percentage of MgO+weight percentage of CaO+weight percentage of SrO) / weight percentage of BaO, and K2 is 0.5-1; Define K3=(weight percentage of MgO+weight percentage of CaO+weight percentage of SrO+weight percentage of BaO+weight percentage of ZnO) / (weight percentage of Na2O+weight percentage of K2O), and K3 is 0.6-1.

2. A method for preparing ultra-thin glass, characterized in that: The method includes: (1) contacting and mixing the components of the composition according to claim 1 to obtain a mixture; (2) subjecting the mixed material to melt treatment I and melt treatment II in sequence to obtain a molten material; wherein the temperature of the melt treatment I is lower than the temperature of the melt treatment II; (3) The molten material is sequentially molded, annealed, thinned and chemically strengthened.

3. The method according to claim 2, characterized in that In step (2), the temperature of the melt treatment I is 50-100°C lower than the temperature of the melt treatment II; and / or In step (2), the conditions of the melt treatment I include at least: a temperature of 1550-1580°C and a time of 3-5 hours; and / or In step (2), the conditions of the melt treatment II include at least: a temperature of 1600-1650°C and a time of 4-6 hours.

4. The method according to claim 3, characterized in that In step (2), the temperature of the melt treatment I is 60-80°C lower than the temperature of the melt treatment II.

5. Ultra-thin glass prepared by the method described in any one of claims 2 to 4.

6. Use of the ultra-thin glass according to claim 5 in preparing a flexible cover plate.