Josephson junction and method for preparing the same

By forming a through channel on the substrate and performing tilt evaporation, the Josephson junction is prepared using a low-resolution UV lithography mechanism, the problem of high cost and low output in the existing technology is solved, and the low output is achieved Cost and high yield preparation effect.

CN116156999BActive Publication Date: 2024-11-15ORIGIN QUANTUM COMPUTING TECH (HEFEI) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211186715.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-15
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

The prior art cannot effectively utilize low-resolution UV lithography mechanism to prepare the Josephson junction, resulting in high manufacturing costs and low output.

Method used

By forming a photoresist layer with a through-channel on the substrate and tiltingly deposition along the channel direction, vertically overlapping superconducting lines are formed, and the Josephson junction is prepared by using a low-resolution UV lithography mechanism to reduce photolithography resolution requirements of the machine.

Benefits of technology

The Josephson junction is prepared using low-resolution UV lithography mechanism, reducing manufacturing costs and increasing yields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116156999B_ABST
    Figure CN116156999B_ABST
Patent Text Reader

Abstract

The present invention discloses a Josephson junction and a preparation method thereof. The preparation method comprises: providing a substrate, forming a first photoresist layer on the substrate, the first photoresist layer having a first channel penetrating therethrough, the first channel including an upper channel and a lower channel having a width greater than that of the upper channel, the upper channel being located above the opening of the lower channel; performing oblique evaporation in a direction perpendicular to the first channel, forming a first superconducting wire parallel to the first channel and at least partially located in a shielding area on the substrate in the first channel; stripping the first photoresist layer, forming a second photoresist layer on the substrate, the second photoresist layer having a second channel having the same structure as the first channel and perpendicular to the first channel; forming a barrier layer on the surface of the first superconducting wire in the second channel; performing oblique evaporation in a direction perpendicular to the second channel, forming a second superconducting wire vertically overlapping the barrier layer and at least partially located in a shielding area on the substrate in the second channel. The present invention can prepare a Josephson junction using a low-resolution UV lithography machine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor process technology, and in particular to a Josephson junction and a preparation method thereof. Background Art

[0002] Superconducting quantum chips are electronic circuits based on Josephson junctions, which usually include resonant cavities, control circuits, readout circuits, "air bridges" and Josephson junctions. Except for the Josephson junction, the line widths of the remaining structures are all in the micron size, and can all be exposed in batches using relatively inexpensive low-resolution ultraviolet (UV) lithography machines. The size of the Josephson junction is usually at the submicron level, such as 200nm×200nm. Due to the limited resolution of the UV lithography machine, it is impossible to complete the exposure of a 200nm line width. Therefore, the existing process can only use electron beam exposure equipment or high-resolution deep ultraviolet (DUV) lithography machines to prepare the Josephson junction, or modify the ultraviolet (UV) lithography machine to improve its resolution.

[0003] However, the exposure speed of electron beam lithography equipment is very slow, which limits the mass production of quantum chips; the equipment price and maintenance cost of deep ultraviolet (DUV) lithography equipment are very high; the transformation of ultraviolet (UV) lithography equipment requires a very high level of technology, and the resolution improvement is limited. Therefore, the existing Josephson junction preparation process is costly and has low yield. Summary of the invention

[0004] The purpose of the present invention is to provide a Josephson junction and a preparation method thereof, so as to solve the problem that the low-resolution UV lithography machine in the prior art cannot prepare the Josephson junction. The Josephson junction can be prepared by using the low-resolution UV lithography machine, which can reduce the manufacturing cost of the Josephson junction and improve its output.

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a Josephson junction, comprising:

[0006] Providing a substrate, forming a first photoresist layer on the substrate, wherein the first photoresist layer has a first channel penetrating therethrough, the first channel comprising an upper channel and a lower channel having a width greater than that of the upper channel, the upper channel being located above an opening of the lower channel so that the substrate in the lower channel is partially blocked;

[0007] Performing oblique evaporation in a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area;

[0008] Stripping the first photoresist layer to form a second photoresist layer on the substrate, wherein the second photoresist layer has a second channel having the same channel structure as the first channel and perpendicular to the first channel;

[0009] forming a barrier layer on the surface of the first superconducting wire in the second channel;

[0010] Oblique evaporation is performed along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel, which is perpendicularly overlapped with the barrier layer and at least partially located in the shielding area.

[0011] Preferably, the first photoresist layer and the second photoresist layer both include a first photoresist sublayer and a second photoresist sublayer stacked from bottom to top, the lower channel is located in the first photoresist sublayer, and the upper channel is located in the second photoresist sublayer.

[0012] Preferably, the dissolution rate of the first photoresist sub-layer in the developer is higher than that of the second photoresist sub-layer, or the sensitivity of the first photoresist sub-layer to light is higher than that of the second photoresist sub-layer.

[0013] Preferably, the first superconducting wire and the second superconducting wire are all located in the shielding area.

[0014] Preferably, before the step of forming a barrier layer on the surface of the first superconducting wire in the second channel, the method further comprises:

[0015] An ion beam etching process is used to etch the natural oxide layer on the surface of the first superconducting wire in the second channel, and the etching angle of the natural oxide layer is the same as the coating angle of the inclined evaporation.

[0016] Preferably, the preparation method further comprises:

[0017] The second photoresist layer is stripped off.

[0018] Preferably, the barrier layer is formed by oxidation.

[0019] Preferably, the step of performing inclined evaporation along a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area further comprises:

[0020] Physical bombardment is performed along a direction parallel to the first channel to remove coating residues on the substrate exposed in the upper channel of the first channel, wherein the coating residues are generated during the oblique evaporation.

[0021] Preferably, the step of performing inclined evaporation along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel that is parallel to the second channel and at least partially located in the shielding area further comprises:

[0022] Physical bombardment is performed in a direction parallel to the second channel to remove the plating residue on the substrate exposed in the upper channel of the second channel.

[0023] Preferably, the physical bombardment adopts an ion beam etching process, a reactive ion etching process, a plasma cleaning process or a bias cleaning process.

[0024] Preferably, the step of performing physical bombardment in a direction parallel to the first channel comprises:

[0025] Performing a first physical bombardment along a direction parallel to the first channel at a first inclination angle;

[0026] A second physical bombardment is performed along a direction parallel to the first channel at a second tilt angle, and the sum of the first tilt angle and the second tilt angle is 180 degrees.

[0027] Preferably, the step of performing physical bombardment in a direction parallel to the second channel comprises:

[0028] Performing a first physical bombardment along a direction parallel to the second channel at the first tilt angle;

[0029] A second physical bombardment is performed along a direction parallel to the second channel at the second tilt angle.

[0030] In order to solve the above technical problems, the present invention also provides a Josephson junction obtained according to any of the preparation methods described above.

[0031] Different from the prior art, the preparation method of the Josephson junction provided by the present invention forms two photoresist layers on a substrate in sequence, the two photoresist layers both have a lower channel and an upper channel exposing the substrate, the width of the lower channel is greater than the width of the upper channel, and the channel directions of the two photoresist layers are perpendicular to each other, and the two photoresist layers are respectively subjected to inclined evaporation to form two vertically overlapping superconducting wires on the substrate, and a Josephson junction is obtained at the overlapping portion. Due to the use of inclined evaporation, the line width of the superconducting wire is smaller than the width of the upper channel, and only a photolithography machine is required to expose the upper channel, and the requirements for the resolution of the photolithography machine are relatively low, so that the Josephson junction can be prepared by using a low-resolution UV photolithography machine, and the low-resolution UV photolithography machine is low in price and fast in exposure speed, so the manufacturing cost of the Josephson junction can be reduced and its yield can be increased.

[0032] The Josephson junction provided by the present invention and the method for preparing the Josephson junction belong to the same inventive concept, and therefore have the same beneficial effects, which will not be described in detail herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A schematic flow chart of a method for preparing a Josephson junction provided in an embodiment of the present invention.

[0034] Figure 2a~2h The figure is a schematic diagram of the process of preparing a Josephson junction according to an embodiment of the present invention.

[0035] Figure 3 for Figure 2a Cross-sectional view in the AA direction.

[0036] Figure 4 Schematic diagram of the principle of inclined evaporation.

[0037] Figure 5 Schematic diagram of the principle of physical bombardment.

[0038] Explanation of the reference numerals: 1-substrate, 2-first photoresist layer, 21-first channel, 211-upper channel, 212-lower channel, 21A-first photoresist sublayer, 21B-second photoresist sublayer, 3-first superconducting wire, 31, 61-plating residues, 4-second photoresist layer, 41-second channel, 5-barrier layer, 6-second superconducting wire. DETAILED DESCRIPTION

[0039] The specific implementation of the present invention will be described in more detail below in conjunction with the schematic diagram. The advantages and features of the present invention will become clearer from the following description and claims. It should be noted that the drawings are all in a very simplified form and are not in exact proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.

[0040] In the description of the present invention, it is necessary to understand that the terms "center", "up", "down", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0042] refer to Figure 1 The embodiment of the present invention provides a method for preparing a Josephson junction, the method comprising the following steps:

[0043] S1: providing a substrate and forming a first photoresist layer on the substrate, wherein the first photoresist layer has a first channel extending therethrough, the first channel comprising an upper channel and a lower channel having a width greater than that of the upper channel, the upper channel being located above an opening of the lower channel so that the substrate in the lower channel is partially blocked.

[0044] For example, Figure 2a , is a top view of the structure after the first photoresist layer is formed on the substrate. A first photoresist layer 2 is formed on the substrate 1, and the first photoresist layer 2 has a first channel 21. It should be noted that the first photoresist layer 2 is only schematically shown in part in the figure. In the actual process, the first photoresist layer 2 can completely cover the substrate 1. Figure 3 As shown, the first channel 21 includes an upper channel 211 and a lower channel 212, the upper channel 211 and the lower channel 212 are connected, the upper channel 211 is located above the opening of the lower channel 212, the upper channel 211 penetrates to the upper surface of the first photoresist layer 2, and the lower channel 212 penetrates to the lower surface of the first photoresist layer 2, thereby exposing the substrate 1. The width of the lower channel 212 is greater than the width of the upper channel 211, so that the cross-sectional shape of the first channel 21 forms a "convex" shape. When forming the first channel 21, the highest resolution of the photolithography machine only needs to be able to expose and develop the upper channel 211.

[0045] S2: performing oblique evaporation in a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area.

[0046] For example, Figure 2b , is a top view of the structure after the first superconducting wire is formed on the substrate. When the inclined evaporation is performed, the coating material at least partially enters the shielded area of ​​the substrate 1 in the first channel 21, and finally forms the first superconducting wire 3. The coating material is usually aluminum. It should be noted that in order to show the position of the first superconducting wire 3, Figure 2b The first superconducting wire 3 is processed for perspective, but it does not mean that the first photoresist layer 2 is transparent, nor does it mean that the first superconducting wire 3 is located above the first photoresist layer 2. If there are subsequent figures with the same situation, they will not be explained one by one.

[0047] In this embodiment, the first superconducting wire 3 is entirely located in the shielding area. Due to the use of inclined coating, the line width of the first superconducting wire 3 is affected by the coating angle. Figure 4As shown, the dotted line with an arrow indicates the coating direction of the coating material. Assuming that the width of the upper trench 211 is L, the width of the shielding area is D, the thickness of the upper trench 211 is h1, the thickness of the lower trench 212 is h2, the coating angle is θ1, and the line width of the first superconducting wire 3 is d, then the line width d=Lx, where x=h1 / tanθ1, so d=L-h1 / tanθ1, so the line width of the first superconducting wire 3 is related to the width of the upper trench 211, the thickness of the upper trench 211, and the coating angle. By adjusting L, h1 and θ1, the line width of the first superconducting wire 3 can be controlled. When the width and thickness of the upper trench 211 remain unchanged, the smaller the coating angle, the smaller the line width of the first superconducting wire 3. The thickness h2 of the lower trench 212 and the width D of the shielding area can be set according to actual needs, as long as they do not hinder the coating.

[0048] Since the highest resolution of the lithography machine does not need to reach the line width of the first superconducting wire 3, but only needs to reach the width of the upper trench 211, the cost of the lithography machine can be reduced. For example, assuming that the line width of the first superconducting wire 3 is 200nm, the coating angle is 60 degrees, and the thickness of the upper trench 211 is 1000nm, then it can be calculated that the width of the upper trench 211 is about 777nm, so the highest resolution of the lithography machine only needs to reach 777nm to produce a superconducting wire with a line width of 200nm.

[0049] S3: stripping the first photoresist layer to form a second photoresist layer on the substrate, wherein the second photoresist layer has a second channel having the same channel structure as the first channel and perpendicular to the first channel.

[0050] For example, Figure 2d , is a top view of the structure after the second photoresist layer is formed on the substrate. After the first photoresist layer 2 is peeled off, the first superconducting wire 3 is left, and then the second photoresist layer 4 is formed on the substrate 1. It should be noted that the second photoresist layer 4 is only partially schematically shown in the figure. In the actual process, the second photoresist layer 4 can completely cover the substrate 1. The second photoresist layer 4 has a second channel 41. The second channel 41 has the same structure as the first channel 21, but is perpendicular to the first channel 21. Similarly, when forming the second channel 41, the highest resolution of the photolithography machine only needs to meet the upper channel that can expose and develop the second channel 41.

[0051] S4: forming a barrier layer on the surface of the first superconducting wire in the second channel.

[0052] The barrier layer can be formed by oxidation. By controlling the gas pressure and time during oxidation, the thickness of the barrier layer can be adjusted, thereby adjusting the resistance of the Josephson junction. For example, Figure 2e4 is a top view of the structure after a barrier layer is formed on the surface of the first superconducting wire.

[0053] S5: performing oblique evaporation along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel that is perpendicularly overlapped with the barrier layer and at least partially located in the shielding area.

[0054] For example, Figure 2f , is a top view of the structure after the second superconducting wire is formed on the substrate. After the inclined evaporation is performed again, the coating material at least partially enters the shielded area of ​​the substrate 1 in the lower trench, and finally forms the second superconducting wire 6, and the second superconducting wire 6 overlaps vertically with the barrier layer 5, thereby forming a superconducting layer-barrier layer-superconducting layer structure at the overlap, and obtaining a Josephson junction. In this embodiment, the second superconducting wire 6 is entirely located in the shielded area.

[0055] In order to facilitate the subsequent processes, in this embodiment, the preparation method further includes:

[0056] S6: stripping the second photoresist layer. Figure 2h , which is a top view of the structure after the second photoresist layer 4 is stripped off. After the second photoresist layer 4 is stripped off, only the first superconducting wire 3 and the second superconducting wire 6 are left on the substrate 1.

[0057] In order to facilitate the formation of the first channel and the second channel, in some embodiments of the present invention, the first photoresist layer and the second photoresist layer both include a first photoresist sublayer and a second photoresist sublayer stacked from bottom to top, the lower channel is located in the first photoresist sublayer, and the upper channel is located in the second photoresist sublayer. The first channel or the second channel is obtained by exposing and developing the first photoresist sublayer and the second photoresist sublayer. Furthermore, in order to better control the width of the upper channel and the lower channel, in this embodiment, the dissolution rate of the first photoresist sublayer in the developer is higher than that of the second photoresist sublayer, or the sensitivity of the first photoresist sublayer to light is higher than that of the second photoresist sublayer, so that the width of the lower channel is greater than the width of the upper channel during exposure or development. Please refer again Figure 4 The lower channel 212 is located in the first photoresist sublayer 21A, and the upper channel 211 is located in the second photoresist sublayer 21B. The thickness of the lower channel 212 is the thickness of the first photoresist sublayer 21A, and the thickness of the upper channel 211 is the thickness of the second photoresist sublayer 21B.

[0058] In some embodiments of the present invention, when the second photoresist layer is exposed to the atmosphere during the formation process, a natural oxide layer will be formed on the surface of the first superconducting wire. The thickness of the natural oxide layer is uncontrollable and will affect the resistance of the Josephson junction. Therefore, the natural oxide layer needs to be removed before the barrier layer is formed. In order to remove the natural oxide layer, before the step of forming the barrier layer on the surface of the first superconducting wire in the second channel, it also includes: using an ion beam etching process to etch the natural oxide layer on the surface of the first superconducting wire in the second channel, and the etching angle of the natural oxide layer is the same as the coating angle of the oblique evaporation. Exemplarily, the natural oxide layer can be etched using an ion beam etcher integrated in the high vacuum chamber of an electron beam evaporation device, and the etching angle is the same as the coating angle of the oblique evaporation, so that the first superconducting wire surface in the second channel and in the second channel shielding area can be etched. Figure 2d As shown, after forming the second photoresist layer 4 and before forming the barrier layer 5 on the surface of the first superconducting wire 3, ion beam etching needs to be performed along a direction perpendicular to the second channel to remove the natural oxide layer on the surface of the first superconducting wire 3 in region B.

[0059] In some embodiments of the present invention, the step of performing oblique evaporation along a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area, that is, step S2, also includes: performing physical bombardment along a direction parallel to the first channel to remove the coating residue on the substrate exposed in the upper channel of the first channel, the coating residue is generated during the oblique evaporation. When the oblique evaporation is performed, the metal vapor will diverge and produce coating residue on the substrate directly below the upper channel. The coating residue is composed of scattered metal particles with a very thin thickness and is not conductive to each other. The coating residue may affect the performance of the Josephson junction, so it needs to be removed. Figure 2b As shown in FIG. 2 , when the first superconducting wire 3 is formed, a plating residue 31 is generated on the substrate 1 directly below the upper trench 211. Figure 2c , which is a top view of the structure after removing the plating residue in the first channel. After forming the first superconducting wire 3 and before stripping the first photoresist layer 2, the plating residue 31 is removed after physical bombardment in a direction parallel to the first channel 21.

[0060] Further, the step of performing inclined evaporation along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel that is parallel to the second channel and at least partially located in the shielding area, that is, step S5, further includes: performing physical bombardment along a direction parallel to the second channel to remove the coating residue on the substrate exposed in the upper channel of the second channel. Figure 2f As shown in FIG. 1 , when the second superconducting wire 6 is formed, a plating residue 61 is generated on the substrate 1 directly below the upper trench. Figure 2g, which is a top view of the structure after removing the plating residue in the second channel. After forming the second superconducting wire 6 and before stripping the second photoresist layer 4, the plating residue 61 is removed after physical bombardment in a direction parallel to the second channel 41.

[0061] Exemplarily, a specific method is that the physical bombardment adopts an ion beam etching process, a reactive ion etching process, a plasma cleaning process or a bias cleaning process.

[0062] In order to completely remove the coating residues and avoid the coating residues remaining, in this embodiment, the step of performing physical bombardment along a direction parallel to the first channel includes:

[0063] Performing a first physical bombardment along a direction parallel to the first channel at a first inclination angle;

[0064] A second physical bombardment is performed along a direction parallel to the first channel at a second tilt angle, and the sum of the first tilt angle and the second tilt angle is 180 degrees.

[0065] For example, Figure 5 As shown, the two physical bombardments use an ion beam etching process, and the projection of the ion beam on the substrate 1 is parallel to the first trench 21. The solid line with an arrow in the figure indicates the direction of the ion beam, and the dotted line indicates the projection of the ion beam on the substrate 1. During the first physical bombardment, the angle between the ion beam and the substrate 1 is the first tilt angle θ2, and during the second physical bombardment, the angle between the ion beam and the substrate 1 is the second tilt angle (180°-θ2). The directions of the two physical bombardments are opposite to each other. In this way, the coating residue directly below the upper trench 211 of the first trench 21 can be completely removed.

[0066] Similarly, physical bombardment along a direction parallel to the second channel includes:

[0067] Performing a first physical bombardment along a direction parallel to the second channel at a first tilt angle;

[0068] A second physical bombardment is performed along a direction parallel to the second channel at a second tilt angle.

[0069] In the above manner, the method for preparing the Josephson junction of the present embodiment forms a first photoresist layer having a first channel, performs oblique evaporation in a direction perpendicular to the first channel to form a first superconducting wire with a smaller line width, then peels off the first photoresist layer and forms a second photoresist layer having a second channel, and after forming a barrier layer on the surface of the first superconducting wire, performs oblique evaporation again in a direction perpendicular to the second channel to form a second superconducting wire with a smaller line width, thereby obtaining a Josephson junction at the intersection of the first superconducting wire and the second superconducting wire. Since the formation of the superconducting wire has a low requirement on the resolution of the lithography machine, a high-resolution lithography machine is not required, so that the Josephson junction can be prepared using a low-resolution UV lithography machine. The low-resolution UV lithography machine is cheap and has a fast exposure speed, so the manufacturing cost of the Josephson junction can be reduced and its output can be increased.

[0070] The embodiment of the present invention also protects a Josephson junction, which is obtained by using the preparation method of the above embodiment.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example" or "specific example" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0072] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A method for preparing a Josephson junction, characterized in that: include: Providing a substrate, forming a first photoresist layer on the substrate, wherein the first photoresist layer has a first channel penetrating therethrough, the first channel comprising an upper channel and a lower channel having a width greater than that of the upper channel, the upper channel being located above an opening of the lower channel so that the substrate in the lower channel is partially blocked; Performing oblique evaporation in a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area; Stripping the first photoresist layer to form a second photoresist layer on the substrate, wherein the second photoresist layer has a second channel having the same channel structure as the first channel and perpendicular to the first channel; forming a barrier layer on the surface of the first superconducting wire in the second channel; Oblique evaporation is performed along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel, which is perpendicularly overlapped with the barrier layer and at least partially located in the shielding area.

2. The preparation method according to claim 1, characterized in that: The first photoresist layer and the second photoresist layer each include a first photoresist sublayer and a second photoresist sublayer stacked from bottom to top, the lower channel is located in the first photoresist sublayer, and the upper channel is located in the second photoresist sublayer.

3. The preparation method according to claim 2, characterized in that: The dissolution rate of the first photoresist sub-layer in the developer is higher than that of the second photoresist sub-layer, or the sensitivity of the first photoresist sub-layer to light is higher than that of the second photoresist sub-layer.

4. The preparation method according to claim 1, characterized in that: The first superconducting wire and the second superconducting wire are all located in the shielding area.

5. The preparation method according to claim 1, characterized in that: Before the step of forming a barrier layer on the surface of the first superconducting wire in the second channel, the method further comprises: An ion beam etching process is used to etch the natural oxide layer on the surface of the first superconducting wire in the second channel, and the etching angle of the natural oxide layer is the same as the coating angle of the inclined evaporation.

6. The preparation method according to claim 1, characterized in that: The preparation method further comprises: The second photoresist layer is stripped off.

7. The preparation method according to claim 1, characterized in that: The barrier layer is formed by oxidation.

8. The preparation method according to claim 1, characterized in that: The step of performing inclined evaporation along a direction perpendicular to the first channel to form a first superconducting wire on the substrate in the first channel that is parallel to the first channel and at least partially located in the shielding area also includes: Physical bombardment is performed along a direction parallel to the first channel to remove coating residues on the substrate exposed in the upper channel of the first channel, wherein the coating residues are generated during the oblique evaporation.

9. The preparation method according to claim 8, characterized in that: The step of performing inclined evaporation along a direction perpendicular to the second channel to form a second superconducting wire on the substrate in the second channel that is parallel to the second channel and at least partially located in the shielding area also includes: Physical bombardment is performed in a direction parallel to the second channel to remove the plating residue on the substrate exposed in the upper channel of the second channel.

10. The preparation method according to claim 9, characterized in that: The physical bombardment adopts an ion beam etching process, a reactive ion etching process, a plasma cleaning process or a bias cleaning process.

11. The preparation method according to claim 9 or 10, characterized in that: The step of performing physical bombardment in a direction parallel to the first channel comprises: Performing a first physical bombardment along a direction parallel to the first channel at a first inclination angle; A second physical bombardment is performed along a direction parallel to the first channel at a second tilt angle, and the sum of the first tilt angle and the second tilt angle is 180 degrees.

12. The preparation method according to claim 11, characterized in that: The step of performing physical bombardment in a direction parallel to the second channel comprises: Performing a first physical bombardment along a direction parallel to the second channel at the first tilt angle; A second physical bombardment is performed along a direction parallel to the second channel at the second tilt angle.

13. A Josephson junction obtained according to the preparation method according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Preparation method of superconducting Josephson junction

    CN111403590A

  • Josephson junction preparation method, device and equipment and superconducting device

    CN113257989A

  • Tunnel junction element, and manufacturing method thereof

    JP2007227407A