A kind of organic binder for vanadium-titanium magnetite pellets and its use method
By using fine-grained dry powder organic binder composed of carboxymethyl starch, carboxymethyl cellulose sodium and borax, the problems of poor adhesion and poor ball-forming performance of vanadium titanium magnetite pellets are solved, and the pellets are improved Strength and grade meet the requirements for blast furnace use and reduce costs.
Patent Information
- Application Number
- CN202211585380.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-09
AI Technical Summary
The existing vanadium titanium magnetite pellet adhesives have problems such as poor adhesion, poor ball formation performance, low thermal stability, high rebate rate and poor economic benefits, resulting in lowering of iron concentrate pellet grade and blast furnace use The requirement was not met.
The fine-grained dry powder organic binder consisting of carboxymethyl starch, carboxymethyl cellulose sodium and borax is used to moisten and pelletize and control the particle size distribution, and increase the drop strength and burst temperature of the raw balls. And oxidized pellets of vanadium titanium magnetite are prepared under suitable roasting conditions.
It significantly reduces the amount of binder added to iron concentrate pellets, improves the grade and strength of finished pellets, meets the requirements for use of medium and large blast furnaces, and reduces the residual amount of binder and production costs.
Smart Images

Figure BDA0003991959780000041 
Figure BDA0003991959780000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vanadium-titanium magnetite agglomeration, and particularly relates to an organic binder for vanadium-titanium magnetite pellets and a use method thereof. Background Art
[0002] Iron ore oxide pellets offer excellent metallurgical properties and improve the permeability of blast furnace charge columns, making them considered a high-quality charge essential for optimizing blast furnace charge structure. Binders are essential raw materials for the production of iron ore concentrate pellets. The basic principles for selecting a pelletizing binder include: ① excellent bonding and ball-forming properties; ② the green pellets produced should exhibit good resistance to thermal cracking, as well as high compressive and drop strength; and ③ the binder should minimize impact on the iron grade of the finished pellets. Currently, the vast majority of pelletizing plants, both domestically and internationally, use bentonite as a binder, typically at a dosage of 2%-3% and sometimes as high as 5%. Production practice has demonstrated that the majority of the bentonite remains in the finished pellets after roasting, reducing their TFe grade. For every 1% of bentonite added, the iron grade decreases by 0.6%-0.7%.
[0003] There are also many organic binders used in the preparation of oxidized pellets in China, such as sodium carboxymethyl starch mentioned in the document "Mechanism of Sodium Carboxymethyl Starch in Improving Pellet Strength" (Journal of Central South University of Technology 2001, 32(4): 390-393); modified cellulose in the document "Organic Binders Replacing Bentonite to Prepare Oxidized Pellets" (Journal of Central South University of Technology 2007, 38(5): 850-856); polyacrylamide in the document "Study on Synthetic Organic Polymer Binders in Magnetite Concentrate Powder Agglomeration" (Metal Mines 2001, 11: 27-30); study on extraction process factors in the preparation of HA series pellet binders (Sintering Pellets 1998, 23(6): 21-24); and humic acid and sodium alginate mentioned in the patent "A Cheap and High-Efficiency Binder for Pellets and Its Preparation Method" (Publication No. CN101230416A). However, due to the complexity of the properties of iron ore concentrate and the high production cost of binders, these purely organic binders still have many problems in pellet production. Organic binders have not been widely used for many reasons, the main reasons can be divided into the following: 1) The binder is too sticky, making it difficult to add or mix evenly in industrial production; 2) The binder has poor ball-forming properties, making it difficult to control the pellet size and the pelletizing rate low; 3) The binder pellets have poor thermal stability, low burst temperature, high return rate, and difficult to carry out industrial production; 4) The finished pellets have low strength and cannot meet the requirements of blast furnace use; 5) The price is too high, resulting in poor economic benefits. Summary of the Invention
[0004] In order to overcome the defects of the above-mentioned prior art, the present invention provides an organic binder for vanadium-titanium magnetite pellets with low usage and small residual amount, which can significantly reduce the amount of binder added to iron concentrate pellets and improve the grade of the finished pellets; the organic binder is a fine-grained dry powder, which is easy to add and mix, and can be used for the production of vanadium-titanium magnetite pellets, and can also be promoted and applied to ordinary iron concentrate pellets. It can improve the drop strength and burst temperature of green pellets; and make the strength of the finished pellets reach more than 2000N, thereby meeting the use requirements of medium and large blast furnaces.
[0005] In order to achieve the above-mentioned purpose of the invention, the present invention provides an organic binder for vanadium-titanium magnetite pellets, which consists of carboxymethyl starch, sodium carboxymethyl cellulose and borax, wherein the mass percentage of carboxymethyl starch is 45-55%, the mass percentage of sodium carboxymethyl cellulose is 45-55%, and the mass percentage of borax is 3-8%.
[0006] The content of the organic binder-0.074mm particle size is ≥99%, the water content of the carboxymethyl starch is ≤9%, and the water content of the sodium carboxymethyl cellulose is ≤10%.
[0007] A method for using the above-mentioned organic binder for vanadium-titanium magnetite pellets, the method comprising the following steps:
[0008] ① Vanadium titanomagnetite and 0.5% by mass of bentonite are mixed and then grinded to obtain a mixed material A, in which the content of vanadium titanomagnetite-0.074mm is 65-73% and the content of bentonite-0.074mm is 90-100%; the finer the particle size, the better the sphericity.
[0009] ② The organic binder (0.1-0.28% by mass of the vanadium-titanium magnetite) is mixed with the mixed material A to obtain a mixed material B; the -0.074mm particle size content of the mixed material B is greater than or equal to 86%, and the -0.045mm particle size content is greater than or equal to 35%; the finer the overall particle size, the more conducive it is to material ball formation, the more appropriate the particle size distribution is, and it is beneficial to improve the quality of the raw balls.
[0010] ③Put the mixed material B into balls on a disc ball making machine for 16 minutes, and control the moisture content of the balls to 8-10%;
[0011] ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C;
[0012] ⑤ Preheat the dry ball C obtained in step ④ at 900-1000° C. for 12-20 minutes, and then calcine at 1200-1300° C. for 12-20 minutes to obtain vanadium-titanium magnetite oxide pellets.
[0013] Compared with the existing technology, the beneficial effects of the present invention are as follows: the present invention overcomes the defects of the traditional process that completely uses bentonite as a binder, resulting in a large residual amount and reducing the TFe grade of the pellets; the organic binder used in the vanadium-titanium magnetite pellets is low in dosage and small in residual amount, which can significantly reduce the amount of binder added to the iron concentrate pellets and improve the grade of the finished pellets. The organic binder is a fine-grained dry powder that is easy to add and mix. It can be used in the production of vanadium-titanium magnetite pellets and can also be promoted and applied to ordinary iron concentrate pellets. It can significantly improve the drop strength and burst temperature of vanadium-titanium magnetite green balls; at the same time, it also overcomes the problem of low pellet strength after the application of other organic binders, and significantly improves the strength of the finished pellets to more than 2000N / piece, thereby meeting the use requirements of medium and large blast furnaces. The organic binder for vanadium-titanium magnetite pellets is low in price and can make the pellets have good metallurgical properties, so it has broad market prospects. DETAILED DESCRIPTION
[0014] The present invention is further described below with reference to specific examples, but is not intended to limit the present invention in any way. To avoid further elaboration, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified. The performance of the pellets was tested in accordance with the standards GB / T 14201-2018 "Determination of compressive strength of iron pellets for blast furnaces and direct reduction", YB / T4696-2018 "Vanadium-titanium iron pellets", and GB / T 27692-2011 "Acidic iron pellets for blast furnaces".
[0015] Example 1
[0016] An organic binder for vanadium-titanium magnetite pellets comprises: 45% by mass of carboxymethyl starch, 52% by mass of sodium carboxymethyl cellulose, and 3% by mass of borax, which are configured into an organic binder CD and then set aside.
[0017] The method for using the organic binder for vanadium-titanium magnetite pellets comprises the following steps:
[0018] ① Mixing vanadium titanomagnetite and 0.5% by weight of bentonite and then grinding them to obtain a mixed material A, wherein the vanadium titanomagnetite-0.074mm content is 65% and the bentonite-0.074mm content is 97%;
[0019] ② The organic binder CD (0.28% by weight of the vanadium-titanium magnetite) was mixed with the mixed material A to obtain a mixed material B; the mixed material B had a -0.074 mm particle size content of 86% and a -0.045 mm particle size content of 35%;
[0020] ③ Make balls of mixed material B on a disc ball making machine for 16 minutes, and control the moisture content of the balls to 8-10%. After the balls are made, measure the drop strength, compressive strength and burst temperature of the balls.
[0021] ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C;
[0022] ⑤ Preheat the dry ball C obtained in step ④ at 950° C. for 20 min, and then calcine at 1250° C. for 20 min to obtain vanadium-titanium magnetite oxide pellets.
[0023] The performance indicators of the green balls and vanadium-titanium magnetite oxide pellets prepared in Example 1 are shown in Table 1.
[0024] Example 2
[0025] An organic binder for vanadium-titanium magnetite pellets comprises: 45% by mass of carboxymethyl starch, 52% by mass of sodium carboxymethyl cellulose, and 3% by mass of borax, which are configured into an organic binder CD and then set aside.
[0026] The method for using the organic binder for vanadium-titanium magnetite pellets comprises the following steps:
[0027] ① Vanadium titanomagnetite and 0.5% by mass of bentonite were mixed and then ground to obtain a mixed material A, in which the vanadium titanomagnetite-0.074mm content was 73% and the bentonite-0.074mm content was 97%;
[0028] ② The organic binder CD (0.28% by weight of the vanadium-titanium magnetite) was mixed with the mixed material A to obtain a mixed material B; the mixed material B had a -0.074 mm particle size content of 87% and a -0.045 mm particle size content of 36%;
[0029] ③ Make balls of mixed material B on a disc ball making machine for 16 minutes, and control the moisture content of the balls to 8-10%. After the balls are made, measure the drop strength, compressive strength and burst temperature of the balls.
[0030] ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C;
[0031] ⑤ Preheat the dry ball C obtained in step ④ at 950° C. for 20 min, and then calcine at 1250° C. for 20 min to obtain vanadium-titanium magnetite oxide pellets.
[0032] The performance indicators of the green balls and vanadium-titanium magnetite oxide pellets prepared in Example 2 are shown in Table 1.
[0033] Example 3
[0034] An organic binder for vanadium-titanium magnetite pellets comprises: 45% by mass of carboxymethyl starch, 52% by mass of sodium carboxymethyl cellulose, and 3% by mass of borax, which are configured into an organic binder CD and then set aside.
[0035] The method for using the organic binder for vanadium-titanium magnetite pellets comprises the following steps:
[0036] ① Vanadium titanomagnetite and 0.5% by mass of bentonite were mixed and then ground to obtain a mixed material A, in which the vanadium titanomagnetite-0.074mm content was 69% and the bentonite-0.074mm content was 98%;
[0037] ② The organic binder CD (0.28% by weight of the vanadium-titanium magnetite) was mixed with the mixed material A to obtain a mixed material B; the mixed material B had a -0.074 mm particle size content of 88% and a -0.045 mm particle size content of 37%;
[0038] ③ Make balls of mixed material B on a disc ball making machine for 16 minutes, and control the moisture content of the balls to 8-10%. After the balls are made, measure the drop strength, compressive strength and burst temperature of the balls.
[0039] ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C;
[0040] ⑤ Preheat the dry ball C obtained in step ④ at 950° C. for 20 min, and then calcine at 1250° C. for 20 min to obtain vanadium-titanium magnetite oxide pellets.
[0041] The performance indicators of the green balls and vanadium-titanium magnetite oxide pellets prepared in Example 3 are shown in Table 1.
[0042] Table 1 Performance indexes of green balls and vanadium-titanium magnetite oxidation pellets
[0043]
[0044] Comparative Example 1
[0045] The method of preparing vanadium-titanium magnetite oxide pellets using bentonite as a binder comprises the following steps:
[0046] ① Vanadium titanomagnetite and 2% by mass of bentonite were mixed and then ground to obtain a mixed material A, in which the content of vanadium titanomagnetite-0.074mm was 69% and the content of bentonite-0.074mm was 98%.
[0047] ③ The mixed material A is pelletized on a disc pelletizer for 16 minutes, and the moisture content of the raw balls is controlled at 8-10%. After the balls are pelletized, the drop strength, compressive strength and burst temperature of the raw balls are measured.
[0048] ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C.
[0049] ⑤ Preheat the dry ball C obtained in step ④ at 950° C. for 20 min, and then calcine at 1250° C. for 20 min to obtain vanadium-titanium magnetite oxide pellets.
[0050] The performance indicators of the green balls and vanadium-titanium magnetite oxide pellets prepared in Comparative Example 1 are shown in Table 2.
[0051] Table 2 Performance indexes of green balls and vanadium-titanium magnetite oxidation pellets
[0052]
[0053] Comparing the test results in Table 1 and Table 2, it can be seen that the green ball falling and bursting temperatures of the 2% bentonite pellets are lower than those of the bentonite pellets of the present invention, and do not meet the requirements for industrial use; and the binder dosage is higher than that of the present invention.
[0054] Anyone skilled in the art will be able to utilize the above-disclosed technical content to make many possible changes and modifications to the technical solution of the present invention, or to modify it into equivalent embodiments with equivalent changes, without departing from the scope of the technical solution of the present invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention that do not depart from the content of the technical solution of the present invention shall still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for using an organic binder for vanadium-titanium magnetite pellets, characterized in that: The method of use comprises the following steps: ① Mix vanadium-titanium magnetite and 0.5% by mass of bentonite and grind them to obtain a mixed material A; wherein the content of -0.074 mm of the vanadium-titanium magnetite is 65% to 73%, and the content of -0.074 mm of the bentonite is 90% to 100%; ② Mixing the organic binder with a mass percentage of 0.1% to 0.28% of the vanadium-titanium magnetite with the mixed material A to obtain a mixed material B; the -0.074 mm particle content of the mixed material B is ≥86%, and the -0.045 mm particle content is ≥35%; ③ Make balls of mixed material B on a disc ball making machine for 16 minutes, and control the moisture content of the balls to 8%~10%; ④ Dry the green balls obtained in step ③ at 105°C to obtain dry balls C; ⑤ Preheating the dry ball C obtained in step ④ at 900°C-1000°C for 12-20 min, and then roasting at 1200°C-1300°C for 12-20 min to obtain vanadium-titanium magnetite pellets; The organic binder consists of carboxymethyl starch, sodium carboxymethyl cellulose and borax; wherein the mass percentage of carboxymethyl starch is 45% to 55%, the mass percentage of sodium carboxymethyl cellulose is 45% to 55%, and the mass percentage of borax is 3% to 8%.
2. The method for using the organic binder for vanadium-titanium magnetite pellets according to claim 1, characterized in that: The organic binder-0.074 mm particle size content is ≥99%.
3. The method for using the organic binder for vanadium-titanium magnetite pellets according to claim 1, characterized in that: The water content of the carboxymethyl starch is ≤9%, and the water content of the sodium carboxymethyl cellulose is ≤10%.
Citation Information
Patent Citations
Cheap highly effective binder for pellet ore and preparation method thereof
CN101230416A
A process for separating iron from other metals in iron containing feed stocks
CA2623628A1
Method for producing oxidized pellet using organic binder fully instead of bentonite
CN101423892A
Binder for coke powder molding and application method thereof
CN101760276A
Acidic full-vanadium-titanium pellets and preparation method thereof
CN102220486A