Metal nanoparticles and framework heteroatom molecular sieve composite catalytic material and preparation method and application thereof
By introducing heteroatoms and metal precursors during the synthesis process of molecular sieves, and using silanization reagents to fix and disperse metal elements, a composite catalytic material of metal oxide nanoparticles and molecular sieves is formed, which solves the problem of insufficient catalytic activity in the existing technology and achieves It achieves efficient catalysis of macromolecular reactants, especially high conversion rate and selectivity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
Patent Information
- Application Number
- CN202111424579.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The existing preparation process cannot achieve the synergistic catalytic effect of highly dispersed metal nanoparticles in molecular sieves and hierarchical pore molecular sieves at the same time, resulting in insufficient catalytic activity, especially poor catalytic performance for macromolecular reactants.
By introducing heteroatom precursors and metal element precursors during the synthesis process of molecular sieves, and using the coordination groups of silanization reagents to fix and disperse metal elements, a composite catalytic material of metal oxide nanoparticles and molecular sieves is formed. The alkyl chain support layer expands the pores to achieve uniform dispersion and cooperative catalysis of metal nanoparticles in the channels of multi-stage molecular sieves.
The specific surface area, pore volume and macromolecular reactivity of the composite catalytic material are improved. The synergistic catalytic effect between the metal oxide nanoparticles and the heteroatoms in the framework significantly improves the catalytic activity for macromolecular substrates, such as in cyclooctane. High conversion rates and selectivities were obtained in the co-oxidation reaction of alkenes and isobutyraldehyde.
Smart Images

Figure CN116174015B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a composite catalytic material of metal nanoparticles and framework heteroatom molecular sieves, and a preparation method and application thereof. Background Art
[0002] In recent years, researchers at home and abroad have replaced Si or Al in the molecular sieve framework with transition metal elements or main group elements such as Ge, Ti, B, P, Fe, Ga, and Zr to form heteroatom molecular sieves. The introduction of heteroatoms into the molecular sieve framework has a significant effect on the modulation of the molecular sieve's physical properties such as pore structure, surface acidity, and particle size. Traditional molecular sieves have weak surface acidity and weak catalytic ability, but after the introduction of heteroatoms into the molecular sieve framework structure, the physical and chemical properties of the molecular sieve are modulated, the number and activity of the molecular sieve active sites are increased, its catalytic activity is improved, and the molecular sieve is endowed with special catalytic properties, which broadens its application areas.
[0003] Due to the limitation of pores, microporous molecular sieves can only be diffused by reactants and oxides of small molecular size, and thus cannot catalyze reactions involving large molecules. To address this defect, mesopores are introduced into microporous molecular sieves, and even the molecular sieves with multi-level pores are further expanded, thereby improving the performance of microporous molecular sieves when applied to large molecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include the removal of skeleton atoms, the double template synthesis method of ordered micro-mesoporous composite molecular sieves, the hard template method, the dry gel conversion method, and the silanization method. Among them, the silanization method is a relatively simple and widely used method.
[0004] Direct hydrothermal synthesis generally refers to the direct introduction of metal precursors during the crystallization of molecular sieves. During the hydrothermal crystallization process, the metal precursors can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structural units, the metal nanoparticles are evenly embedded in the molecular sieve framework. Since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursors are very easy to form hydroxide precipitation. To solve this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.). In addition to preventing coagulation, the complexing agent can also play the role of isolation and dispersion, which helps to form highly dispersed metal nanoparticles. Highly dispersed metal nanoparticles help to inhibit the sintering of metals at high temperatures.
[0005] However, the two technical effects of complexing metal precursors with organic ligands and then introducing them into the hydrothermal crystallization process of the molecular sieve to make the nanoparticles highly dispersed in the molecular sieve crystals, and using the silanization method to prepare multi-level pore molecular sieves and exert the synergistic catalytic effect of the framework heteroatom sites and the metal nanoparticles in the molecular sieve pores, cannot be achieved simultaneously by the existing preparation processes. Summary of the invention
[0006] The purpose of the present disclosure is to provide a metal oxide nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have uniform particle size and are evenly dispersed in the molecular sieve pores and play a synergistic catalytic role with heteroatoms in the framework.
[0007] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a metal oxide nanoparticle and molecular sieve composite catalytic material, comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, wherein the metal element M is a metal element capable of forming a stable oxide aggregate; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium.
[0008] Optionally, the composite catalytic material has the following XPS characteristics:
[0009] The electron binding energy of the metal element M in the composite catalyst material is denoted as T1,
[0010] The electron binding energy of the metal element M in the stable oxide aggregate is denoted as T2;
[0011] T0 defined by the following formula (1) is any value between 0.03% and 0.2%;
[0012] T0=(T1-T2) / T2 Formula (1);
[0013] Preferably, the T0 is any value between 0.05 and 0.19%.
[0014] Optionally, the framework heteroatom molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0015] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; preferably selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum and copper;
[0016] Preferably, the metal M is Co, and the stable oxide aggregate is Co3O4 aggregate;
[0017] The metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0018] The metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0019] The metal M is Ni, and the oxide aggregate is NiO aggregate;
[0020] The metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0021] The metal M is Pt, and the oxide aggregate is a PtO2 aggregate; or
[0022] The metal M is Cu, and the oxide aggregate is CuO aggregate;
[0023] When the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2 When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2 When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
[0024] Optionally, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.002-0.04):1;
[0025] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.002-0.1):1.
[0026] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65ml / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-11nm.
[0027] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising the following steps:
[0028] S1, mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a hydrolysis solution;
[0029] S2, mixing the metal element M precursor and the hydrolysis solution to obtain a first mixed material;
[0030] S3, adding a silanization agent to the first mixed material, and mixing to obtain a reaction mixture;
[0031] S4, performing hydrothermal crystallization and calcination treatment on the reaction mixture;
[0032] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.
[0033] Optionally, the molar ratio of the silicon source calculated as Si element: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal M element: the silanization agent is 1: (0.001~1): (0.001~0.05): (5~100): (0.001~0.2): (0.025~0.4), preferably 1: (0.005~0.5): (0.001~0.05): (5~100): (0.001~0.2): (0.025~0.3).
[0034] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0035] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0036]
[0037] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0038] Optionally, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0039] wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl;
[0040] Further preferably, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0041] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0042] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0043] Optionally, in step S1, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain the hydrolysis solution;
[0044] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0045] Optionally, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of a chloride, a nitrate or a sulfate of a heteroatom element; the inorganic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C):
[0046]
[0047] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0048] Optionally, R5, R6, R7 and R8 are each independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl;
[0049] Preferably, when the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is boron, the skeleton heteroatom precursor is selected from one or more of boric acid and borate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is aluminum, the skeleton heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; when the skeleton heteroatom is phosphorus, the skeleton heteroatom precursor is selected from one or more of orthophosphoric acid, triethyl phosphoric acid and metaphosphate; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
[0050] Optionally, in step S2, the metal element M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal element M precursor is a water-soluble inorganic salt of the metal element M;
[0051] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0052] Preferably, the metal element M precursor is an aqueous solution of the metal element M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal element M precursor is 1:(50-500).
[0053] Optionally, in step S3, the general formula of the silanization agent is R9Si(R10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the carbon number of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer from 1 to 18, and the carbon number of the aromatic group is any integer from 6 to 18;
[0054] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; more preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane;
[0055] Preferably, the mixing conditions in step S3 include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0056] Optionally, in step S4, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0057] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0058] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0059] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0060] Through the above technical scheme, the present disclosure provides a metal oxide nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The metal nanoparticle and molecular sieve composite material provided by the present disclosure is prepared by introducing a heteroatom precursor into the reaction mixture of molecular sieve synthesis, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces a metal element precursor and a silanization agent into the reaction mixture. The coordination group complex metal of the silanization agent plays a role in fixing and dispersing the metal element. The alkyl chain in the silanization agent also has a supporting layer to achieve a pore expansion effect. The molecular sieve of the prepared composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle size and are evenly dispersed in the pores of the multi-level pore heteroatom framework molecular sieve. The metal elements of the metal oxide particles and the heteroatoms in the framework can play a synergistic catalytic role, effectively improving the catalytic activity of the composite catalytic material for macromolecular substrates.
[0061] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0063] Figure 1 This is the SEM image of the product prepared in Example 1.
[0064] Figure 2 The XRD spectrum of the product prepared in Example 1 is shown.
[0065] Figure 3-1 This is the TEM image of the product prepared in Example 1.
[0066] Figure 3-2 This is the TEM image of the product prepared in Example 1.
[0067] Figure 4 This is the FT-IR spectrum of the product prepared in Example 1.
[0068] Figure 5 This is the UV-Vis graph of the product prepared in Example 1.
[0069] Figure 6 This is the Co spectrum of XPS of the product prepared in Example 1.
[0070] Figure 7 This is the XPS Ti spectrum of the product prepared in Example 1. DETAILED DESCRIPTION
[0071] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0072] The inventors of the present disclosure surprisingly found through a large number of experiments that heteroatom precursors, metal element M precursors and silanization agents (including at least one coordination group complexed with the metal element M) are introduced into the reaction raw materials of the crystallized synthetic molecular sieve, and after hydrothermal crystallization and calcination, heteroatoms can be introduced into the molecular sieve framework, and the skeleton heteroatom molecular sieve of the composite catalytic material has a large specific surface area and pore volume, the metal oxide nanoparticles have a high uniformity of particle size and can be evenly dispersed in the skeleton heteroatom molecular sieve pores, and the heteroatom metal sites on the molecular sieve framework and the metal sites (nanoparticles) of the metal element M in the pores can achieve a synergistic catalytic effect. The composite material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins, for example, when used in the co-oxidation reaction of cyclooctene and isobutyraldehyde, a high cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.
[0073] The first aspect of the present disclosure provides a metal oxide nanoparticle and molecular sieve composite catalytic material, comprising a skeleton heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, wherein the metal element M is a metal element capable of forming a stable oxide aggregate; the skeleton heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the skeleton of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is selected from one or more of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium.
[0074] The present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, wherein the molecular sieve of the composite material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore heteroatom framework molecular sieve. There is an obvious interaction between the metal elements of the metal oxide particles and the heteroatoms in the framework. After the heteroatoms are introduced into the molecular sieve framework, the two metal sites in the composite material can play a synergistic catalytic role, effectively improving the catalytic activity of the composite catalytic material for macromolecular substrates.
[0075] In the present disclosure, stable oxide aggregates refer to the oxide aggregates of the metal element M known in the art that can exist most stably in the natural state. For example, when the metal M is Co, the stable oxide aggregates are Co3O4 aggregates; when the metal M is Cu, the stable oxide aggregates are CuO aggregates.
[0076] The inventors of the present disclosure also found that compared with the XPS binding energy of the metal M element in the stable oxide aggregate, the XPS binding energy of the metal M element introduced in the composite material of the present disclosure has changed, and the heteroatoms in the skeleton can also affect the XPS binding energy of the metal M element in the composite material. When the XPS chemical binding energy of the metal element M in the composite material changes within a certain range compared with the XPS chemical binding energy of the metal element M in its stable oxide, the composite material can obtain a higher cyclooctene conversion rate and epoxycyclooctene selectivity.
[0077] In one embodiment, the composite catalytic material has the following XPS characteristics:
[0078] The electron binding energy of the metal element M in the composite catalyst material is denoted as T1,
[0079] The electron binding energy of the metal element M in the stable oxide aggregate is denoted as T2;
[0080] T0 defined by the following formula (1) is any value between 0.03% and 0.2%;
[0081] T0 = (T1 - T2) / T2 Formula (1).
[0082] In a preferred embodiment, the T0 is any value between 0.05% and 0.19%. When the T0 of the composite catalyst material is within this range, the composite catalyst material has higher catalytic activity, cyclooctene conversion rate and epoxycyclooctene selectivity.
[0083] In one embodiment, the framework heteroatom molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0084] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold. In a preferred embodiment, the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum and copper.
[0085] In an optional embodiment, the metal M is Co, and the stable oxide aggregate is a Co3O4 aggregate;
[0086] In an optional embodiment, the metal M is Mn, and the oxide aggregate is a MnO2 aggregate;
[0087] In an optional embodiment, the metal M is Fe, and the oxide aggregate is Fe2O3 aggregate;
[0088] In an optional embodiment, the metal M is Ni, and the oxide aggregate is NiO aggregate;
[0089] In an optional embodiment, the metal M is Pd, and the oxide aggregate is a PdO aggregate;
[0090] In an optional embodiment, the metal M is Pt, and the oxide aggregate is a PtO2 aggregate;
[0091] In an optional embodiment, the metal M is Cu, and the oxide aggregate is CuO aggregate;
[0092] When the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2 When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2 When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
[0093] 2p in XPS characteristics 3 / 2 Taking electrons as an example, the specific meaning is: 2p represents 2p orbital, and 3 / 2 represents the spin-orbit coupling quantum number.
[0094] In one embodiment, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1, preferably (0.002-0.04):1;
[0095] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.002-0.1):1.
[0096] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 11 nm, preferably 0.5 to 10 nm; the BET specific surface area is 400 to 800 m 2 / g, preferably 400 to 700 m 2 / g; total pore volume is 0.3-0.65 ml / g, preferably 0.31-0.63 ml / g; micropore volume is 0.1-0.19 mL / g, preferably 0.11-0.18 mL / g; mesopore volume is 0.2-0.46 mL / g, preferably 0.21-0.46 mL / g. The composite catalytic material disclosed in the present invention has a multi-level pore structure, which is conducive to catalyzing the reaction of macromolecular substrates.
[0097] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising the following steps:
[0098] S1, mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a hydrolysis solution;
[0099] S2, mixing the metal element M precursor and the hydrolysis solution to obtain a first mixed material;
[0100] S3, adding a silanization agent to the first mixed material, and mixing to obtain a reaction mixture;
[0101] S4, performing hydrothermal crystallization and calcination treatment on the reaction mixture;
[0102] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.
[0103] The present invention introduces heteroatom precursors into the reaction mixture for synthesizing molecular sieves, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present invention also introduces metal element precursors and silanization agents into the reaction mixture, and the coordination group of the silanization agent complexes the metal to fix and disperse the metal element, and the supporting layer of the long-chain alkane has a pore expansion effect; and the metal M oxide nanoparticles formed by the metal M introduced during the molecular sieve synthesis process can also be uniformly dispersed in the pores of the multi-level pore molecular sieve.
[0104] In one embodiment, in step S1, the molar ratio of the silicon source calculated as Si element: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal M element: the silanization agent is 1: (0.001-1): (0.001-0.05): (5-100): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-0.5): (0.001-0.05): (5-100): (0.001-0.2): (0.025-0.3).
[0105] Specifically, the water used in step S1 can be water commonly used in synthesizing molecular sieves. In order to avoid the introduction of heteroatoms, deionized water is preferred.
[0106] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
[0107] In one embodiment, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;
[0108] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):
[0109]
[0110] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0111] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0112] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0113] In a further preferred embodiment, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0114] Wherein R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0115] In a preferred embodiment, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0116] In another preferred embodiment, the molecular sieve in the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0117] In another preferred embodiment, the molecular sieve in the composite catalyst material is a Beta molecular sieve, and the template is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0118] In one embodiment, in step S1, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution;
[0119] The conditions for the hydrolysis and alcohol removal treatment include: stirring hydrolysis at 0-95°C for 2-10 hours; preferably stirring hydrolysis at 50-95°C for 2-8 hours; wherein the hydrolysis and alcohol removal treatment makes the mass content of alcohol produced by hydrolysis of the organosilicon source in the hydrolysis solution less than 10 ppm.
[0120] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal element (such as a compound containing the metal element and / or a metal element) can achieve the purpose of the present disclosure.
[0121] In one embodiment, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of a chloride, a nitrate or a sulfate of a heteroatom element; the inorganic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C):
[0122]
[0123] wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R5, R6, R7 and R8 are independently selected from a straight-chain alkyl group having 2 to 4 carbon atoms and a branched-chain alkyl group having 2 to 4 carbon atoms;
[0124] Optionally, R5, R6, R7 and R8 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl or isohexyl; preferably, they are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
[0125] In an optional embodiment, the skeleton heteroatom is titanium, and the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; in an optional embodiment, the skeleton heteroatom is boron, and the skeleton heteroatom precursor is selected from one or more of boric acid and borate; in an optional embodiment, the skeleton heteroatom is tin, and the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide. In one optional embodiment, the framework heteroatom is aluminum, and the framework heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; in one optional embodiment, the framework heteroatom is phosphorus, and the framework heteroatom precursor is selected from one or more of orthophosphoric acid, triethylphosphoric acid and metaphosphate; in one optional embodiment, the framework heteroatom is germanium, and the framework heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide (such as ethanol germanium, isopropoxide germanium), germanium chloride and sodium germanate.
[0126] In one embodiment, in step S2, the metal element M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal element M precursor is a water-soluble inorganic salt of the metal element M;
[0127] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0128] Preferably, the metal element M precursor is an aqueous solution of the metal element M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal element M precursor is 1:(50-500).
[0129] In one embodiment, in step S3, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer in the range of 1 to 18, preferably any integer in the range of 1 to 12; the number of carbon atoms of the aromatic group can be any integer in the range of 6 to 18, preferably any integer in the range of 6 to 12.
[0130] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0131] In the present disclosure, different silanization agents can be selected for different metal elements M. For example, when the metal element M is Co, the silanization agent is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; when the metal element M is Au, the silanization agent is at least one of 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane and 3-mercaptobutyltrimethoxysilane.
[0132] In one embodiment, in step S4, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0133] In one embodiment, in step S4, the conditions of the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0134] The third aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves prepared according to the method described in the second aspect of the present disclosure.
[0135] The fourth aspect of the present disclosure provides the use of the metal oxide nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0136] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.
[0137] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.
[0138] In the present disclosure, the X-ray diffraction (XRD) crystal phase diagram of the sample is measured on a Siemens D5005 X-ray diffractometer, the radiation source is Kα (Cu), and the test range 2θ is 0.5° to 70°.
[0139] The Fourier transform infrared (FT-IR) spectra of the samples were measured on a Nicolet 8210 Fourier transform infrared spectrometer in the range of 400 to 4000 cm -1 .
[0140] The UV-visible diffuse reflectance spectrum (UV-vis) of the samples was measured on a SHIMADZU UV-3100 UV-visible spectrometer in the range of 400 to 4000 cm -1 .
[0141] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0142] The transmission electron microscopy (TEM) images of the samples were obtained using a FEI Tecnai G2F20S-TWIN transmission electron microscope.
[0143] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0144] The XPS characterization of the samples was carried out on an ESCALAB 250 X-ray photoelectron spectrometer with monochromatic Al Kα X-rays, an energy of 1486.6 eV, a power of 150 W, and the C1s peak (284.8 eV) of contaminated carbon was used to correct the nuclear charge shift.
[0145] The cobalt nitrate in the following examples is all cobalt nitrate hexahydrate.
[0146] Example 1
[0147] (1) 1.63 g of 25.05 wt% tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol), 0.170 g of tetrabutyl titanate (0.0005 mol) and 9 g of water (0.5 mol) were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0148] (2) 0.3 g (0.001 mol) of cobalt nitrate hexahydrate and 1.8 g (0.1 mol) of water were stirred uniformly to obtain a cobalt aqueous solution, and the cobalt aqueous solution was mixed with the hydrolyzed silicon solution obtained in step (1);
[0149] (3) Add 0.56 g of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792, 0.0025 mol) to the mixture of step (2) and stir for 0.5 hour;
[0150] (4) The mixture obtained in step (3) is transferred to a stainless steel closed reactor and crystallized at a constant temperature of 170°C for 28 hours to obtain a sample. The obtained sample is filtered, washed, dried at 120°C for 6 hours, and then calcined in a muffle furnace at 550°C for 6 hours to obtain a metal oxide nanoparticle and molecular sieve composite material product, which is recorded as A-1.
[0151] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of the metal nanoparticles contained in A-1 are listed in Table 2.
[0152] The SEM image of A-1 is as follows Figure 1 The XRD spectrum of A-1 is shown as Figure 2 As shown in Figure 2, XRD analysis shows that it has an MFI structure; TEM of A-1 is as shown in Figure 2 Figure 3-1 and 3-2 The FT-IR spectrum of A-1 is shown in Figure 4; the UV-Vis spectrum of A-1 is shown in Figure 5. Figure 5 The XPS spectrum of A-1 is shown as Figure 6 The peak separation results of the XPS spectrum of A-1 in the range of 455 to 470 eV are shown in Figure 7 shown.
[0153] Among them Figure 1 , Figure 3-1 and 3-2 It can be seen that the product prepared in this example has a regular shape and uniform size, and the molecular sieve as a whole can reach the standard; Figure 4 Medium 960cm -1 The characteristic peaks nearby indicate that Co is bound to the surface of the silicon skeleton; Figure 5 The characteristic peaks around 450-700 nm indicate the interaction between Co and Si; Figure 7 There is a peak of framework Ti at 460.23 eV in the product, which proves that Ti heteroatoms are successfully introduced into the framework of the obtained product.
[0154] Comparative Example 1
[0155] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added, and the obtained product was recorded as D-1. The proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations are referenced to Example 1.
[0156] Comparative Example 2
[0157] This comparative example was prepared according to the method of Example 1, except that no backbone heteroatom precursor was added, and the obtained product was recorded as D-2. The proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations are referenced to Example 1.
[0158] Comparative Example 3
[0159] This comparative example was prepared according to the following method.
[0160] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, tetrabutyl titanate, cobalt acetylacetonate and deionized water were mixed and stirred at 80°C for 8 hours. A first mixture with a molar ratio of SiO2: structure directing agent: TiO2: Co: H2O = 1: 0.2: 0.025: 0.01: 50 was obtained; phenyltriethoxysilane was added to the above first mixture at a molar ratio of SiO2: silanization agent = 1: 0.1, and the stirring was continued for 2 hours. The obtained second mixture was transferred to a pressure-resistant stainless steel reactor; under stirring conditions, it was heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor was cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a titanium silicon molecular sieve encapsulating cobalt. The obtained product was recorded as D-3.
[0161] Embodiments 2 to 9
[0162] The corresponding products A-2 to A-9 were prepared according to the method of Example 1. The proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations refer to Example 1. SEM images of A-2 to A-9 are Figure 1 Similar; XRD analysis shows that it has MFI structure, and the XRD spectrum is similar to Figure 2 Similar; its TEM image is Figure 3-1 and 3-2 Similar; its FT-IR spectrum is Figure 4 Similar; its UV-Vis spectrum is Figure 5 resemblance.
[0163] Example 10
[0164] In this example, a cobalt-containing multi-level porous β molecular sieve was prepared. Referring to the method of Example 1, the ratio and template agent were changed. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product is recorded as A-10.
[0165] Embodiment 11
[0166] In this example, a cobalt-containing multi-level porous MEL molecular sieve was prepared. Referring to the method of Example 1, the ratio and template agent were changed. The template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product is recorded as A-11.
[0167] Example 12
[0168] A multi-level porous MFI molecular sieve containing manganese oxide nanoparticles was prepared, wherein the framework heteroatom was tin, according to the method of Example 1, and the proportions, synthesis conditions and results thereof are shown in Table 1. The obtained product was recorded as A-12.
[0169] Embodiment 13
[0170] The corresponding product was prepared according to the method of Example 1, and its ratio, synthesis conditions and results are shown in Table 1. Other conditions and operations are similar to those of Example 1, and the obtained product is recorded as A-13.
[0171] The hydrothermal crystallization temperature is 140°C and the hydrothermal crystallization time is 7 days; the calcination temperature is 840°C and the calcination time is 9 hours.
[0172] The BET specific surface area, total pore volume, micropore volume and mesopore volume of the products obtained in the above examples and comparative examples, as well as the average particle size of the metal nanoparticles contained in the products are listed in Table 2 below.
[0173] Table 1
[0174]
[0175]
[0176] In Table 1, cobalt nitrate is cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane). The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0177] Table 2
[0178]
[0179] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0180] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding silanization agent), A-1 to A-13 prepared in Examples 1 to 13 of the present disclosure have higher mesopore volume and smaller average particle size of metal nanoparticles, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve, and the degree of aggregation of the metal nanoparticles is lower, the average particle size of the nanoparticles is smaller, and the dispersion is higher.
[0181] Test Case
[0182] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0183] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.
[0184] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):
[0185]
[0186]
[0187]
[0188] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and the samples were taken for analysis. The results are shown in Table 3.
[0189] Table 3
[0190]
[0191]
[0192] In the present disclosure, the T2 value of Co3O4, a stable oxide aggregate of the metal element Co, is 781.25 eV; the T2 value of MnO2, a stable oxide aggregate of manganese, is 642.10 eV.
[0193] According to the data in Table 3, compared with the products D-1 to D-3 obtained in Comparative Example 1 (no silanization agent added), Comparative Example 2 (no skeleton heteroatom precursor added) and Comparative Example 3 (preparation method is different from the present disclosure), the T0 of the products A-1 to A-13 obtained in Examples 1 to 13 of the present disclosure is between 0.03 and 0.2%, with higher catalytic activity, cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity. The catalytic activity of the products A-1 to A-13 prepared in Examples 1 to 13 of the present disclosure is higher than that of D-2 without Ti, which also shows that there is a synergistic catalytic effect between the metal element Co and the heteroatom Ti.
[0194] Further comparison of A1-A12 with A-13 shows that, compared with the composite catalytic material A-13, A1-A12 has a T0 of 0.05-0.19%, has higher catalytic activity, and has higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity.
[0195] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0196] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0197] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A composite catalytic material of metal nanoparticles and framework heteroatom molecular sieves, characterized in that: It comprises a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, wherein the metal element M is a metal element capable of forming a stable oxide aggregate, and the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is selected from one or more of titanium, zirconium, tin and germanium; The composite catalytic material has the following XPS characteristics: The electron binding energy of the metal element M in the composite catalyst material is denoted as T1, The electron binding energy of the metal element M in the stable oxide aggregate is denoted as T2; T0 defined by the following formula (1) is any value between 0.03% and 0.2%; T0= (T1-T2) / T2 (1); The metal nanoparticle and framework heteroatom molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a hydrolysis solution; S2, mixing the metal element M precursor and the hydrolysis solution to obtain a first mixed material; S3, adding a silanization agent to the first mixed material, and mixing to obtain a reaction mixture; S4, performing hydrothermal crystallization and calcination treatment on the reaction mixture; Wherein, the skeleton heteroatom precursor comprises the heteroatom element Q; the silanization agent comprises at least one coordination group complexed with the metal element M.
2. According to the composite catalytic material according to claim 1, the T0 is any value between 0.05 and 0.19%.
3. The composite catalytic material according to claim 1, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.
4. The composite catalytic material according to claim 3, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of the following: MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
5. The composite catalytic material according to claim 4, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.
6. The composite catalytic material according to claim 1, characterized in that: The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum and copper.
7. The composite catalytic material according to claim 1, characterized in that: The metal M is Co, and the stable oxide aggregate is Co3O4 aggregate; The metal M is Mn, and the oxide aggregate is a MnO2 aggregate; The metal M is Fe, and the oxide aggregate is Fe2O3 aggregate; The metal M is Ni, and the oxide aggregate is NiO aggregate; The metal M is Pd, and the oxide aggregate is a PdO aggregate; The metal M is Pt, and the oxide aggregate is a PtO2 aggregate; The metal M is Cu, and the oxide aggregates are CuO aggregates; or When the metal element M is Co, Mn, Fe, Ni or Cu, the electron binding energy of the metal element M is 2p 3 / 2 When the metal element M is Pt, the electron binding energy of the metal element M is 4f 7 / 2 When the metal element M is Pd, the electron binding energy of the metal element M is 3d 5 / 2 The binding energy of an electron.
8. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.001-0.05):1; The molar ratio of metal M element to silicon element is (0.001~0.2):
1.
9. The composite catalytic material according to claim 8, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.002-0.04):1; The molar ratio of metal M element to silicon element is (0.002~0.1):
1.
10. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.2~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~11nm.
11. The composite catalytic material according to claim 1, characterized in that: The molar ratio of the silicon source calculated as Si element: template: the skeleton heteroatom precursor calculated as heteroatom element Q: water: metal M element: silanization agent is 1: (0.001~1): (0.001~0.05): (5~100): (0.001~0.2): (0.025~0.4).
12. The composite catalytic material according to claim 11, characterized in that: The molar ratio of the silicon source calculated as Si element: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal M element: the silanization agent is 1: (0.005~0.5): (0.001~0.05): (5~100): (0.001~0.2): (0.025~0.3).
13. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
14. The composite catalytic material according to claim 13, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
15. The composite catalytic material according to claim 14, characterized in that: The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
17. The composite catalytic material according to claim 16, characterized in that: The R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
18. The composite catalytic material according to claim 15, characterized in that: The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
19. The composite catalytic material according to claim 1, characterized in that: The template agent is an organic base.
20. The composite catalytic material according to claim 19, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
21. The composite catalytic material according to claim 20, characterized in that: The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.
22. The composite catalytic material according to claim 21, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.
23. The composite catalytic material according to claim 22, characterized in that: The R1, R2, R3 and R4 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
24. The composite catalytic material according to claim 1, characterized in that The molecular sieve in the composite catalyst material is an MFI molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
25. The composite catalytic material according to claim 1, characterized in that In step S1, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
26. The composite catalytic material according to claim 25, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
27. The composite catalytic material according to claim 1, characterized in that In step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of chloride, nitrate or sulfate of a heteroatom element; the organic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C): (C); wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms.
28. The composite catalytic material according to claim 27, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms.
29. The composite catalytic material according to claim 28, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 2 to 4 carbon atoms and a branched alkyl group having 2 to 4 carbon atoms.
30. The composite catalytic material according to claim 27, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl and isohexyl.
31. The composite catalytic material according to claim 30, characterized in that The R5, R6, R7 and R8 are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
32. The composite catalytic material according to claim 1, characterized in that When the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.
33. The composite catalytic material according to claim 1, characterized in that In step S2, the precursor of the metal element M is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M.
34. The composite catalytic material according to claim 33, characterized in that The metal element M precursor is a water-soluble inorganic salt of the metal element M.
35. The composite catalytic material according to claim 34, characterized in that The metal element M precursor is an aqueous solution of the metal element M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal element M precursor is 1: (50-500).
36. The composite catalytic material according to claim 1, characterized in that In step S3, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amino group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amino group is independently selected from any integer in the range of 1 to 18, and the number of carbon atoms of the aromatic group is any integer in the range of 6 to 18.
37. The composite catalytic material according to claim 36, characterized in that The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
38. The composite catalytic material according to claim 37, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
39. The composite catalytic material according to claim 1, characterized in that The mixing conditions in step S3 include: stirring at 20-80° C. for 0.5-2 hours.
40. The composite catalytic material according to claim 1, characterized in that In step S4, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
41. The composite catalytic material according to claim 40, characterized in that In step S4, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.
42. Use of the metal nanoparticle and framework heteroatom molecular sieve composite catalytic material according to any one of claims 1 to 41 in catalyzing the co-oxidation reaction of aldehydes and olefins.
43. The use according to claim 42, characterized in that The use is the use of the metal nanoparticles and skeleton heteroatom molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.