Composite catalytic material of all-silicon molecular sieve and metal nanoparticles, preparation method and application thereof

By introducing metal precursors, nitrogen-containing ligands and silanization reagents during the synthesis process of molecular sieves, composite catalytic materials of metal nanoparticles and all-silicon molecular sieves are prepared, which solves the problem of insufficient stability and activity of nanometal particles in catalytic reactions. Efficient catalytic activity and hierarchical pore structure are achieved, especially showing excellent catalytic performance in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

CN116174022BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111424562.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-15
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

Existing methods are difficult to simultaneously maintain the high dispersion of nanometal particles and the hierarchical pore structure of molecular sieves during catalytic reactions, resulting in insufficient catalytic activity and stability.

Method used

By introducing metal precursors, nitrogen-containing ligands and silanization reagents during the synthesis process of molecular sieves, and performing hydrothermal crystallization and roasting treatments, composite catalytic materials of metal nanoparticles and all-silicon molecular sieves are prepared to achieve high dispersion of metal particles and molecular sieves. hierarchical pore structure.

Benefits of technology

A metal nanoparticle composite catalytic material with high specific surface area, pore volume and macromolecular reactivity was obtained, which improved the catalytic activity, especially showing high conversion rate and high conversion rate in the co-oxidation reaction of cyclooctene and isobutyraldehyde. Selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174022B_ABST
    Figure CN116174022B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite catalytic material of all-silicon molecular sieve and metal nanoparticles, and a preparation method and application thereof. The composite catalytic material comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the composite catalytic material has the following FT-IR characteristics: the wave number of the FT-IR spectrum of the composite catalytic material is 960cm ‑1 The highest peak intensity in the range is recorded as I1, with a wave number of 800 cm ‑1 The highest peak intensity within the range is recorded as I2, and I0 defined by the following formula (1) is any value between 0.55 and 1.3; I0 = I1 / I2 formula (1). The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have uniform particle size and have a high dispersion in the molecular sieve crystal and on the pore surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a composite catalytic material of all-silicon molecular sieve and metal nanoparticles, and a preparation method and application thereof. Background Art

[0002] The structure and particle size of nano-metal (especially gold and precious metals, etc.) particles, as well as the interaction with the carrier, have a significant regulatory effect on the catalytic reaction. When the particle size of the metal is reduced to below 3nm, it shows a strong catalytic activity for CO oxidation. Since catalytic reactions are often carried out at high temperatures and high pressures, the shape, structure and size of nanoparticles with unique catalytic activity will change in the actual process. Therefore, a key scientific and technological issue in the research and practice of nanocatalysis, especially metal nanoparticle catalysis, is to improve and strengthen the structural stability of nanoparticles under the conditions of catalytic reactions. The methods reported to improve the stability of "nanoparticles" mainly include inert carrier embedding, ligand protection and interaction with the carrier. According to the characteristics of the catalytic reaction, it is required that the active center of the catalytic reaction (generally the metal surface) should be exposed as much as possible while the nanoparticles are stable. The use of porous materials and the geometric and electronic binding characteristics of the porous material channels (generally at the nanometer level) can achieve the purpose of stabilizing the shape, structure and electronic properties of nanoparticles.

[0003] It is a common method to use molecular sieve pores for the loading of nano-metals. On the one hand, due to the small size of the micropores of molecular sieves, and the impregnation method usually uses metal salt solutions for impregnation, the size of metal hydrated ions is generally larger than the pore size of the molecular sieve, and cannot diffuse into the pores, and can only gather on the outer surface of the molecular sieve particles. Therefore, it is difficult to use conventional impregnation methods to highly disperse metal nanoparticles into molecular sieve crystals. Existing methods for introducing metal nanoparticles into molecular sieve crystals include direct synthesis and post-synthesis. Among them, the direct synthesis method generally directly introduces metal precursors during the crystallization process of molecular sieves. During the hydrothermal crystallization process, the metal precursors can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structure units, the metal nanoparticles are evenly embedded in the molecular sieve skeleton.

[0004] On the other hand, due to the limitation of pores, microporous molecular sieves can only be diffused through by reactants of small molecular size, and thus cannot catalyze reactions involving macromolecular substrates. In view of this defect, mesopores or even macropores are introduced into microporous molecular sieves to construct molecular sieves with multi-level pore sizes, thereby improving the performance of microporous molecular sieves when applied to macromolecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include the removal of skeleton atoms, the double template synthesis method of ordered micro-mesoporous composite molecular sieves, the hard template method, the dry gel conversion method and the silanization method. Among them, the silanization method is a relatively simple and widely used method. Since the silanol of the silanization agent hydrolyzes and condenses with the silanol of the molecular sieve precursor to produce a stable Si-O-Si bond, the effect of supporting layer pore expansion can be ensured.

[0005] For example, Wang Baorong et al. (CN 111847471 A) prepared a multi-level porous molecular sieve encapsulating active metals by introducing a silanization agent in a direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very easy to form hydroxide precipitation. In order to solve this problem, the precursor metal ion often forms a complex with a ligand containing a lone pair of electrons (such as an organic amine ligand or ammonia, etc.), such as Wang et al. using ethylenediamine ligands and PdCl2 to form [Pd(NH2CH2CH2NH2)]Cl2 complex precursor, and then directly synthesized a silicalite-1 molecular sieve (Pd@silicalite-1) with uniformly dispersed Pd nanoparticles embedded by a hydrothermal crystallization method.

[0006] In summary, the metal precursors are complexed with organic ligands and then introduced into the hydrothermal crystallization process of the molecular sieve, which can highly disperse the nanoparticles in the molecular sieve crystals; and the introduction of silanization agents into the molecular sieve synthesis process can effectively and simply prepare multi-level pore molecular sieves. The use of silanization agents with coordination groups can further increase the complexation effect and promote the metal to be more located in the mesoporous channels. However, the existing preparation methods are difficult to simultaneously achieve the two effects of highly dispersed metal nanoparticles in the molecular sieve crystals and molecular sieve pore expansion, that is, it is difficult to directly prepare multi-level pore molecular sieves with highly dispersed metal nanoparticles. Summary of the invention

[0007] The purpose of the present disclosure is to provide a composite catalytic material of all-silicon molecular sieve and metal nanoparticles, and its preparation method and application. The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have uniform particle size and have a high dispersion in the molecular sieve crystal and on the pore surface.

[0008] In order to achieve the above-mentioned object, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material in the first aspect, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the composite catalytic material has the following FT-IR characteristics: the wave number of the FT-IR spectrum of the composite catalytic material is 960cm -1 The peak intensity of the highest peak at is recorded as I1, and the wave number is 800cm -1 The peak intensity of the highest peak is recorded as I2; I0 defined by the following formula (1) is any value between 0.55 and 1.3; I0 = I1 / I2 formula (1).

[0009] Optionally, the value of I0 is any value between 0.6 and 1.3.

[0010] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;

[0011] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0012] Optionally, in the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.

[0013] Optionally, the BET specific surface area of ​​the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.16-0.47mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-7nm.

[0014] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nano-oxide particles and molecular sieves, comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture; S2, performing a hydrothermal crystallization treatment and a calcination treatment on the reaction mixture.

[0015] Optionally, in step S1, the molar ratio of silicon source, template, water, metal element M, and silanization agent calculated as SiO2 is 1: (0.001-1): (5-100): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-0.4): (5-100): (0.001-0.15): (0.025-0.3); the molar ratio of nitrogen-containing ligand to metal element M is (0.2-2): 1, preferably (0.5-2): 1.

[0016] Optionally, step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, mixing to obtain a first mixed material; mixing the first mixed material and the silicon hydrolysis solution to obtain a second mixed material; c. adding a silanization agent to the second mixed material, mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.

[0017] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably selected from at least one of organic silicone grease, solid silica gel and white carbon black; further preferably organic silicone grease, the general formula of the organic silicone grease is the structure shown in the following formula (A):

[0018]

[0019] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0020] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):

[0021] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl;

[0022] Further preferably, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0023] The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0024] The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

[0025] Optionally, in step S1, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;

[0026] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.

[0027] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;

[0028] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0029] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0030] Optionally, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; and the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms;

[0031] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0032] Optionally, in step S1, the nitrogen-containing ligand is an alkylamine compound containing only an amino group or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl, and thiol;

[0033] Preferably, the nitrogen-containing ligand is one or more of an alkylamine compound containing only an amino group having a structure shown in the following formula (C), an alcoholamine compound having a structure shown in the following formula (D), and an aminocarboxylic acid compound having a structure shown in the following formula (E):

[0034] R9(NH2) n Formula (C);

[0035] wherein n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms, preferably a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and more preferably one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms, preferably a linear alkylene group having 1 to 6 carbon atoms and a branched alkylene group having 3 to 6 carbon atoms, and more preferably one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene;

[0036] (HOR10 ) m NH (3m) Formula (D);

[0037] Where R 10 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; m is 1, 2 or 3. When m is greater than 1, multiple R 10 Same or different;

[0038] (HOOCR 11 ) x NH (3x) Formula (E);

[0039] Where R 11 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; x is 1, 2 or 3. When x is greater than 1, multiple R 11 Same or different;

[0040] More preferably, the nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.

[0041] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;

[0042] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.

[0043] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.

[0044] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0045] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The present disclosure adds a metal precursor, a nitrogen-containing ligand and a silanization agent to the reaction raw materials of the molecular sieve crystallization synthesis, and the molecular sieve prepared by the composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have a uniform particle size and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalytic material has a high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0046] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0048] Figure 1 This is the FT-IR spectrum of the product prepared in Example 1.

[0049] Figure 2 This is the XRD spectrum of the product prepared in Example 1.

[0050] Figure 3 This is the SEM spectrum of the product prepared in Example 1. DETAILED DESCRIPTION

[0051] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0052] The first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve;

[0053] The composite catalytic material has the following FT-IR characteristics:

[0054] The wave number in the FT-IR spectrum of the composite catalytic material is 960 cm -1 The peak intensity of the highest peak at is recorded as I1, and the wave number is 800cm -1 The peak intensity of the highest peak at is recorded as I2;

[0055] I0 defined by the following formula (1) is any value between 0.55 and 1.3;

[0056] I0=I1 / I2 formula (1).

[0057] The molecular sieve of the composite catalytic material provided by the present invention has a large specific surface area, pore volume and reaction activity of macromolecular substrates; and the molecular sieve of the composite catalytic material has a multi-level pore structure, and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalytic material has high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0058] The inventors of the present disclosure surprisingly found in a large number of experimental studies that when a metal precursor, a nitrogen-containing ligand and a silanization agent are introduced into the molecular sieve synthesis process, after the reaction mixture is subjected to hydrothermal crystallization, washing and calcination, the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has a large specific surface area and pore volume performance, but also the metal oxide nanoparticles have uniform particle size and are evenly dispersed in the molecular sieve crystal (for example, in the molecular sieve mesopores), and may also exist on the surface of the molecular sieve pores; and the inventors also found that the obtained composite catalytic material has a 960cm -1 The highest peak intensity (I1) at 800 cm -1 The ratio of the highest peak intensities (I2) at the locations is related to the catalytic performance of the composite catalytic material, especially when I0 (I0=I1 / I2) satisfies 0.55-1.3, the composite catalytic material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins. For example, when used for the co-oxidation reaction of cyclooctene and isobutyraldehyde, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.

[0059] It should be understood that the term "960 cm" in this disclosure refers to -1 "At 960cm in the infrared spectrum -1 Within a certain range nearby, such as 955-965cm -1 , "800cm -1 "At" means 800cm in the infrared spectrum -1 Within a certain range nearby, such as 795 to 805 cm -1 .

[0060] In a preferred embodiment, the value of I0 is any value between 0.6 and 1.3. When I0 of the composite catalyst material is within this range, it has higher catalytic activity, higher cyclooctene conversion rate and higher cyclooctene oxide selectivity.

[0061] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.

[0062] In one embodiment, the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0063] In one embodiment, the composite catalytic material includes silicon element, metal element M and oxygen element, and the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.15):1.

[0064] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 7 nm, preferably 1 to 6.5 nm, and the BET specific surface area is 400 to 800 m 2 / g, preferably 430 to 800 m 2 / g, the total pore volume is 0.3-0.65 mL / g, preferably 0.31-0.62 mL / g, the micropore volume is 0.1-0.19 mL / g, preferably 0.12-0.18 mL / g, and the mesopore volume is 0.15-0.5 mL / g, preferably 0.16-0.47 mL / g. The composite catalytic material disclosed in the present invention also has a multi-level pore structure, which is conducive to catalyzing large-sized reaction substrates.

[0065] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:

[0066] S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture;

[0067] S2. performing hydrothermal crystallization and calcination on the reaction mixture.

[0068] The present invention introduces a metal precursor, a nitrogen-containing ligand and a silanization agent into the raw materials for the crystallization synthesis of the molecular sieve, which can simultaneously achieve the effects of highly dispersing metal oxide nanoparticles in the molecular sieve crystals and expanding the pores of the molecular sieve support layer, thereby preparing a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.

[0069] In the present disclosure, on the one hand, the metal ions in the reaction mixture are complexed with the nitrogen-containing ligands to achieve the effect of dispersing and stabilizing the metal; at the same time, at least one coordination group of the silanization agent can also be complexed with the metal ions to achieve the effect of fixing and dispersing the metal, so that the metal oxide nanoparticles in the molecular sieve pores obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalyst material. Thus, a multi-level porous all-silicon molecular sieve composite catalyst material with highly dispersed metal nanoparticles is finally prepared.

[0070] In one embodiment, in step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent in terms of SiO2 is 1: (0.001-1): (5-100): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-0.4): (5-100): (0.001-0.15): (0.025-0.3); the molar ratio of nitrogen-containing ligand to metal element M is (0.2-2): 1, preferably (0.5-2): 1. Specifically, the water used in step S1 can be water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.

[0071] In a preferred embodiment, step S1 comprises:

[0072] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;

[0073] b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;

[0074] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.

[0075] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):

[0076]

[0077] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c , R d Each is independently methyl or ethyl.

[0078] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0079] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.

[0080] Further preferably, the template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B):

[0081] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0082] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).

[0083] In a preferred embodiment, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0084] In another preferred embodiment, the molecular sieve of the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0085] In another preferred embodiment, the molecular sieve of the composite catalyst material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves of different structures by selecting different template agents.

[0086] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;

[0087] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.

[0088] Preferably, the hydrolysis-alcohol removal treatment is performed so that the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolysis solution of silicon is less than 10 ppm.

[0089] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.

[0090] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;

[0091] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0092] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0093] In one embodiment, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, preferably 1 to 12 carbon atoms; the number of carbon atoms of the aromatic group can be 6 to 18, preferably 6 to 12;

[0094] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0095] In one embodiment, in step S1, the nitrogen-containing ligand is an alkylamine compound containing only amino groups or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl, and thiol. In the present disclosure, the "alkylamine compound containing only amino groups" means that the alkylamine compound contains only amino groups, which is a nitrogen-containing group, and does not contain other types of nitrogen-containing groups, but the number of amino groups contained can be one or more.

[0096] Preferably, the nitrogen-containing ligand is one or more of an alkylamine compound containing only an amino group having a structure shown in the following formula (C), an alcoholamine compound having a structure shown in the following formula (D), and an aminocarboxylic acid compound having a structure shown in the following formula (E):

[0097] R9(NH2) nFormula (C); wherein n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms, preferably a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and more preferably one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms, preferably a linear alkylene group having 1 to 6 carbon atoms and a branched alkylene group having 3 to 6 carbon atoms, and more preferably one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene;

[0098] (HOR 10 ) m NH (3m) Formula (D); wherein R 10 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; m is 1, 2 or 3. When m is greater than 1, multiple R 10 Same or different;

[0099] (HOOCR 11 ) x NH (3x) Formula (E); wherein R 11 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; x is 1, 2 or 3. When x is greater than 1, multiple R 11 Same or different;

[0100] More preferably, the nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.

[0101] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.

[0102] In one embodiment, in step S2, the calcination temperature is 400-900° C., and the calcination time is 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.

[0103] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.

[0104] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0105] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.

[0106] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.

[0107] The present disclosure will be further described below using examples.

[0108] In the present disclosure, the X-ray diffraction (XRD) crystal phase diagram of the sample is measured on a Siemens D5005 X-ray diffractometer, the radiation source is Kα (Cu), and the test range 2θ is 0.5° to 70°.

[0109] The Fourier transform infrared (FT-IR) spectra of the samples were measured on a Nicolet 8210 Fourier transform infrared spectrometer in the range of 400 to 4000 cm -1 .

[0110] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.

[0111] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.

[0112] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.

[0113] The cobalt nitrate used in the following examples is all cobalt nitrate hexahydrate.

[0114] Example 1

[0115] (1) 1.6 g of 25.05 wt% tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol) and 52.8 g of water (3 mol) were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silicon hydrolysis solution;

[0116] (2) 0.03 g of cobalt nitrate hexahydrate (0.1 mmol) and 0.18 g (0.01 mol) of water were stirred evenly, and then 0.05 mmol of ethylenediamine was added, and the aqueous solution of cobalt was mixed with the hydrolyzed solution of silicon obtained in step (1);

[0117] (3) adding 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stirring for 0.5 hour;

[0118] (4) The mixture obtained in step (3) was transferred to a stainless steel closed reactor and crystallized at a constant temperature of 175° C. for 24 hours to obtain a sample. The obtained sample was filtered, washed, dried at 110° C. for 6 hours, and then calcined in a muffle furnace at 650° C. for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which was recorded as CAT-1.

[0119] The infrared spectrum of CAT-1 is as follows Figure 1 As shown. In the infrared spectrum of this sample, 960cm -1 The peak intensity of the highest peak at 800 cm (absorbance 12%) is -1 The ratio I0 of the peak intensity of the highest peak (absorbance is 15%) is 0.80. The XRD spectrum of CAT-1 is shown in Figure 2 As shown in Figure 1, XRD analysis shows that it has an MFI structure. Figure 3 The BET specific surface area, total pore volume, micropore volume, mesopore volume of CAT-1 and the average particle size of the metal nanoparticles contained therein are listed in Table 2.

[0120] Comparative Example 1

[0121] This comparative example was prepared according to the method of Example 1, except that no nitrogen-containing ligand and silanization agent were added. Other conditions and operations were the same as those of Example 1. The prepared product was recorded as sample DCAT-1.

[0122] Comparative Example 2

[0123] This comparative example was prepared according to patent CN 111847471 A.

[0124] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, cobalt nitrate hexahydrate and deionized water were mixed to obtain a first mixture with a molar ratio of SiO2: structure directing agent: Co: H2O = 1: 0.2: 0.001: 30; then PHAPTMS was added to the above first mixture at a molar ratio of SiO2: silanization agent = 1: 0.025, and after stirring evenly, the obtained second mixture was transferred to a pressure-resistant stainless steel reactor; under stirring conditions, it was heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor was cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous molecular sieve encapsulating cobalt. The prepared product was recorded as sample DCAT-2.

[0125] Comparative Example 3

[0126] This comparative example was prepared according to the method of Ning Wang et al. (JACS, 2016, Vol. 138, pp. 7484-7487).

[0127] First, deionized water was mixed with 13g TPAOH solution and stirred continuously for 10 minutes, and then 8.32g ethyl orthosilicate (0.04mol) was added. After continuous stirring for 6 hours, the mixture became clear after complete hydrolysis. 0.052g cobalt nitrate hexahydrate (0.18mmol, the molar ratio of metal cobalt to silicon source was 0.0045) was dissolved in a mixture of 0.3mL ethylenediamine and 3mL water to prepare [Pd(NH2CH2CH2NH2)2]Cl2 solution, and then the resulting solution was added dropwise to the above mixture and stirred for 30min without precipitation. The reaction mixture was transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and static crystallization was performed at 170°C in a conventional oven for 4 days. The solid product was centrifuged, washed with water and ethanol several times, dried in an oven at 80°C overnight, roasted in an air atmosphere at 550°C for 8 hours, and finally reduced with hydrogen to obtain the product. The prepared product was recorded as sample DCAT-3.

[0128] Embodiment 2 to Embodiment 9

[0129] The corresponding products CAT-2 to CAT-9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations are similar to those of Example 1.

[0130] Example 10

[0131] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, but the ratio and template agent were changed. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as CAT-10.

[0132] Embodiment 11

[0133] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent, and the template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product is recorded as CAT-11.

[0134] Example 12

[0135] The corresponding product was prepared according to the method of Example 1, and its proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1. The obtained product is recorded as CAT-12.

[0136] The hydrothermal crystallization temperature is 110°C and the hydrothermal crystallization time is 6 days; the calcination temperature is 860°C and the calcination time is 9 hours.

[0137] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of metal nanoparticles of the products obtained in the above examples and comparative examples are listed in Table 2 below.

[0138] Table 1

[0139]

[0140] In Table 1, TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane); EDTA is ethylenediaminetetraacetic acid. The reagents used in the present disclosure can be obtained through conventional purchasing channels.

[0141] Table 2

[0142]

[0143] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.

[0144] According to Table 2, compared with DCAT-1 prepared in Comparative Example 1 (without adding nitrogen-containing ligands and silanization agents) and DCAT-3 prepared in Comparative Example 3 (without adding silanization agents), CAT-1 to CAT-12 prepared in Examples 1 to 12 of the present disclosure add silanization agents during the preparation process, and the obtained products have higher mesopore volumes, indicating that the method provided in the present disclosure can effectively expand the pores of molecular sieves.

[0145] Compared with DCAT-2 prepared in Comparative Example 2 (without adding nitrogen-containing ligands), the metal nanoparticles CAT-1 to CAT-12 prepared in the present invention have a smaller average particle size, indicating that the CAT-1 to CAT-12 nanoparticles have a lower degree of aggregation and a higher degree of dispersion.

[0146] Test Case

[0147] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0148] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.

[0149] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):

[0150]

[0151]

[0152]

[0153] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and samples were taken for analysis. The results are shown in Table 3.

[0154] Table 3

[0155]

[0156] According to the data in Table 3, compared with DCAT-1 to DCAT-3 prepared in Comparative Examples 1-3, the I0 of the metal oxide nanoparticles and molecular sieve composite catalytic materials CAT-1 to CAT-12 prepared in Examples 1 to 12 of the present disclosure is between 0.55 and 1.3, and they have higher catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde, and higher cyclooctene conversion rate and epoxycyclooctene selectivity.

[0157] Furthermore, by comparing CAT-1 to 11 with CAT-12, it can be seen that the I0 values ​​of CAT-1 to 11 are any value between 0.6 and 1.30, and CAT-1 to 11 have higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity.

[0158] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0159] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0160] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A metal nanoparticle and molecular sieve composite catalytic material, characterized in that: It comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve, wherein the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following FT-IR characteristics: The wave number in the FT-IR spectrum of the composite catalytic material is 960 cm -1 The peak intensity of the highest peak at is recorded as I1, and the wave number is 800cm -1 The peak intensity of the highest peak at is recorded as I2; I0 defined by the following formula (1) is any value between 0.6 and 1.3; I0= I1 / I2 (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatment; The general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms; The nitrogen-containing ligand is an alkylamine compound containing only an amino group or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl and thiol.

2. The composite catalytic material according to claim 1, characterized in that: The all-silicon molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.

3. The composite catalytic material according to claim 2, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the group consisting of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.

4. The composite catalytic material according to claim 3, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.

5. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):

1.

6. The composite catalytic material according to claim 5, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.15):

1.

7. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of ​​the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.15~0.50mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~7nm.

8. The composite catalytic material according to claim 1, characterized in that: In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.001~1): (5~100): (0.001~0.2): (0.025~0.4); the molar ratio of nitrogen-containing ligand to metal element M is (0.2~2):

1.

9. The composite catalytic material according to claim 8, characterized in that: In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.005~0.4): (5~100): (0.001~0.15): (0.025~0.3); the molar ratio of nitrogen-containing ligand to metal element M is (0.5~2):

1.

10. The composite catalytic material according to claim 1, characterized in that: Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.

11. The composite catalytic material according to claim 10, characterized in that: The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

12. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.

13. The composite catalytic material according to claim 12, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.

14. The composite catalytic material according to claim 13, characterized in that: The silicon source is selected from organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.

15. The composite catalytic material according to claim 14, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.

16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.

17. The composite catalytic material according to claim 16, characterized in that: The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

18. The composite catalytic material according to claim 1, characterized in that: In step S1, the template agent is an organic base.

19. The composite catalytic material according to claim 18, characterized in that: The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

20. The composite catalytic material according to claim 19, characterized in that The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.

21. The composite catalytic material according to claim 20, characterized in that: In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.

22. The composite catalytic material according to claim 21, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from at least one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

23. The composite catalytic material according to claim 1, characterized in that: The molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

24. The composite catalytic material according to claim 10, characterized in that: In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.

25. The composite catalytic material according to claim 24, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.

26. The composite catalytic material according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.

27. The composite catalytic material according to claim 26, characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.

28. The composite catalytic material according to claim 10, characterized in that: The molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).

29. The composite catalytic material according to claim 1, characterized in that: In step S1, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

30. The composite catalytic material according to claim 29, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

31. The composite catalytic material according to claim 1, characterized in that In step S1, the nitrogen-containing ligand is selected from one or more of an alkylamine compound containing only an amino group having a structure represented by the following formula (C), ethanolamine and ethylenediaminetetraacetic acid; R9(NH2) n Formula (C); Wherein, n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms.

32. The composite catalytic material according to claim 31, characterized in that In formula (C), when n is 1, R9 is a straight-chain alkyl group having 1 to 6 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms; when n is 2, R9 is a straight-chain alkylene group having 1 to 6 carbon atoms and a branched-chain alkylene group having 3 to 6 carbon atoms.

33. The composite catalytic material according to claim 32, characterized in that In formula (C), when n is 1, R9 is one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene.

34. The composite catalytic material according to claim 31, characterized in that In step S1, the nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.

35. The composite catalytic material according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.

36. The composite catalytic material according to claim 35, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.

37. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 36 in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins.

38. The use according to claim 37, characterized in that The use includes use of the metal nanoparticles and the molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.