A method for producing a powder metallurgy steel collar

Through specific raw material ratios and production methods, the porosity and surface hardness of the powder metallurgy steel ring are improved, solving the problems of insufficient lubrication performance and air permeability, achieving higher lubrication performance and service life, and reducing production costs. and energy consumption.

CN116174723BActive Publication Date: 2024-10-29LAIWU IRON & STEEL GRP POWDER METALLURGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211392973.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-10-29
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

The oil content of the powder metallurgy steel ring cannot be further increased, and long-term and stable lubricating oil leakage cannot be maintained, which limits the improvement of lubrication performance and service life. At the same time, there is the problem of unsatisfactory air permeability.

Method used

Using specific raw material ratios and production methods, including batching, pressing, sintering, machining and post-processing, through a specific combination of zinc stearate, graphite and cutting agents, the porosity and pore distribution are improved, combining hydrogen and ammonia decomposition gas The mixed atmosphere is used for sintering, and 32# mechanical oil and F5-1 anti-rust oil are used for oil quenching to improve the surface hardness and air permeability of the steel ring.

Benefits of technology

It effectively improves the lubrication performance and service life of the steel ring. The porosity reaches 20-25%, the surface hardness reaches HRA60-63, the air permeability is uniform, the wear is reduced, and the production efficiency and cost are also improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174723B_ABST
    Figure CN116174723B_ABST
Patent Text Reader

Abstract

The present invention provides a production method of a powder metallurgy steel collar, the production method comprising: batching, pressing, sintering, machining, and post-processing; in the mixture obtained by the batching, the weight percentage of each component is: 0.75-0.85% zinc stearate, 0.8-0.9% graphite, 0.5-0.6% cutting agent, and the balance is reduced iron powder. The powder metallurgy steel collar obtained by the production method of the powder metallurgy steel collar effectively improves the porosity and pore distribution of the steel collar, and the oil content exceeds 15%, further improving the lubrication performance of the steel collar during the working process; at the same time, the porosity of the steel collar reaches 20-25%, and the air permeability is uniform throughout the whole circumference; the surface hardness of the steel collar reaches HRA60-63, effectively improving the lubrication performance of the steel collar, effectively reducing the wear of the steel collar during the working process, and effectively improving the service life of the steel collar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel collars, in particular to a production method of a powder metallurgy steel collar. Background Art

[0002] Powder metallurgy mechanical parts refer to mechanical structural parts, sliding bearings, friction materials and other products manufactured by powder metallurgy. Such parts are widely used in the machinery manufacturing industry, especially in household appliances, automobiles, agricultural machinery, engineering machinery, general machinery and other industries. Compared with the same parts manufactured by conventional casting, forging and cutting, the parts manufactured by powder metallurgy have the characteristics of less or no cutting, energy saving, material saving, no environmental pollution, low cost and high efficiency. They can produce materials and products with special properties and other processes that are difficult or impossible to produce. At the same time, due to the good physical and mechanical properties, high design flexibility and low production cost of powder metallurgy parts, they have developed rapidly in recent years, and more and more mechanical parts are produced by powder metallurgy process when designing.

[0003] Steel collars are a type of vulnerable parts with a large consumption in textile machinery. In the prior art, they are generally manufactured by steel stamping, machining, heat treatment, polishing and other processes. The steel collars manufactured in this way have the defects of poor wear resistance and short service life. The biggest feature of powder metallurgy steel collars is that they have many capillary structures. The pores of the capillary pores can store oil. When the steel collar runs at high speed, the lubricating oil stored in the pores continuously seeps out, so that the outer surface of the steel collar is covered with an oil film formed by the lubricating oil seeping out of the pores, thereby playing a role in lubricating and protecting the steel collar, thereby increasing the service life of the steel collar.

[0004] However, the inventors have found through research that the oil content of current powder metallurgy steel collars cannot be further improved, and that long-term stable lubricating oil seepage cannot be maintained, which limits further improvement in the lubrication performance and service life of powder metallurgy steel collars. At the same time, the inventors have also found that existing steel collars still have the problem of unsatisfactory air permeability. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides a production method of a powder metallurgy steel collar, which can effectively improve the oil content of the powder metallurgy steel collar, maintain long-term stable lubricating oil seepage, further improve its lubrication performance and service life, and at the same time improve the air permeability of the powder metallurgy steel collar.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for producing a powder metallurgy steel collar, the method comprising: batching, pressing, sintering, machining, and post-processing;

[0008] The mixed material comprises taking 50-60% of the total amount of reduced iron powder, mixing it with zinc stearate, graphite and cutting agent, and mixing them evenly; adding the remaining amount of reduced iron powder, mixing and batching, and then passing through an 80-mesh sieve to obtain a mixed material;

[0009] In the mixture, the weight percentage of each component is: zinc stearate 0.75-0.85%, graphite 0.8-0.9%, cutting agent 0.5-0.6%, and the balance is reduced iron powder;

[0010] The mixed material is pressed, sintered, machined and post-processed to obtain a powder metallurgy steel collar.

[0011] Preferably, the reduced iron powder has a bulk density of 2.52 g / cm 3 , flow rate is 30S / 50g, compressibility at 490MPa is ≥6.55g / cm 3 .

[0012] Preferably, the graphite is of model LC-325-999; and the cutting agent is MnS cutting agent.

[0013] Furthermore, the powder metallurgy steel collar has a surface hardness of HRA60-63, an oil content of more than 15%, and a porosity of 20-25%.

[0014] Furthermore, the pressing comprises pressing the mixed material into a shape to obtain a blank;

[0015] The pressing density is controlled at 6.2-6.4 g / cm 3 ;

[0016] The density uniformity of the blank is not greater than 0.1 g / cm 3 .

[0017] Furthermore, the sintering method is to place the pressed blank in a sintering atmosphere, sinter and dewax for 40-50 minutes at a temperature of 680-690°C; then sinter for 40-50 minutes at a temperature of 980-990°C; after sintering, when the blank is cooled to 100-110°C, immerse it in treatment oil for 10-20 minutes to obtain a sintered part.

[0018] Preferably, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas;

[0019] The volume ratio of the hydrogen to the ammonia decomposition gas is 1:9-10.

[0020] Preferably, the treatment oil is composed of 32# machine oil and F5-1 anti-rust oil;

[0021] The weight ratio of the 32# machine oil to the F5-1 anti-rust oil is 6:4-6.

[0022] Furthermore, the machining is to cut the sintered part obtained by sintering to obtain a cutting part;

[0023] During the machining process, cubic boron nitride machining blades are used to cut the sintered part.

[0024] Furthermore, the post-processing includes oil quenching the machined cutting piece for 30-40 minutes, and then finishing it for 40-50 minutes to obtain a powder metallurgy steel collar;

[0025] The temperature of the oil quenching treatment is 840-850°C.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The powder metallurgy steel collar production method of the present invention effectively improves the porosity and pore distribution of the steel collar by matching specific raw materials and combining a specific production method. The pores on the surface of the prepared steel collar are not closed, and the oil content of the steel collar exceeds 15%, further improving the lubrication performance of the steel collar during operation.

[0028] (2) The production method of the powder metallurgy steel collar of the present invention, by matching specific raw materials and combining a specific production method, the porosity of the steel collar produced reaches 20-25%. The generation of bubbles is qualitatively detected, and the air permeability of the steel collar is uniform all around, and the air permeability of each part is uniform and good, and the performance of the steel collar is stable.

[0029] (3) The powder metallurgy steel collar production method of the present invention can produce a steel collar with a surface hardness of HRA60-63. During its working process, the steel collar has good air permeability and a uniform surface oil film, which effectively improves the lubrication performance of the steel collar, effectively reduces the wear of the steel collar during its working process, and effectively increases the service life of the steel collar.

[0030] (4) Compared with the existing steel collar production method, the powder metallurgy steel collar production method of the present invention is easier to cut, has high production efficiency, and reduces production costs by 10%. At the same time, it effectively reduces the sintering temperature and reduces production energy consumption by about 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a metallographic image (50X) of the powder metallurgy steel collar prepared in Example 1. DETAILED DESCRIPTION

[0032] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0033] Example 1

[0034] A method for producing a powder metallurgy steel collar is as follows:

[0035] 1. Ingredients

[0036] Take 50% of the total amount of iron powder, mix it with zinc stearate, graphite and cutting agent, and mix them evenly; add the remaining amount of iron powder and continue mixing for 40 minutes. After mixing for 20 minutes, pass it through an 80-mesh sieve to obtain a mixture.

[0037] The iron powder is 100% FHY80.25 reduced iron powder produced by Luyin New Materials, with a bulk density of 2.52 g / cm 3 , flow rate 30S / 50g, compressibility ≥6.55g / cm 3 (490MPa).

[0038] The zinc stearate has a melting point of 122°C.

[0039] The graphite has a model number of LC-325-999.

[0040] The cutting agent is MnS cutting agent.

[0041] In the batching step, the weight percentage of each raw material is as follows: 0.75% zinc stearate, 0.8% graphite, 0.5% cutting agent, and the balance is reduced iron powder.

[0042] 2. Suppression

[0043] The mixture was put into a molding machine and the compaction density was controlled at 6.2 g / cm 3 , pressed into shape, to obtain a blank.

[0044] During the pressing process, the mold is fully demagnetized; and the density uniformity of the blank is not greater than 0.1g / cm 3 .

[0045] 3. Sintering

[0046] The blank is placed on a flat plate in the sintering furnace for sintering, and the number of layers of the product is determined according to the height of the furnace. During the sintering process, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas. The blank is first sintered and dewaxed at 680°C for 40 minutes; then sintered at 980°C for 40 minutes; after sintering, the blank is cooled to 100°C and taken out of the furnace, immersed in treatment oil for 10 minutes to obtain a sintered part.

[0047] The volume ratio of hydrogen to ammonia decomposition gas is 1:9.

[0048] The treatment oil is composed of 32# machine oil and F5-1 anti-rust oil, and the weight ratio of 32# machine oil to F5-1 anti-rust oil is 6:4.

[0049] 4. Machining

[0050] The cutting piece is obtained by cutting the sintered part using a cubic boron nitride machining blade.

[0051] 5. Post-processing

[0052] The cutting parts were subjected to oil quenching treatment for 30 minutes and then polishing treatment for 40 minutes to obtain powder metallurgy steel collars.

[0053] Wherein, the temperature of the oil quenching treatment is 840°C.

[0054] The powder metallurgy steel collar has a surface hardness of HRA63, an oil content of 15.9%, and a porosity of 25%.

[0055] Example 2

[0056] A method for producing a powder metallurgy steel collar is as follows:

[0057] 1. Ingredients

[0058] Take 55% of the total amount of iron powder and mix it with zinc stearate, graphite and cutting agent. After mixing evenly, add the remaining amount of iron powder and continue mixing for 45 minutes. After mixing for 25 minutes, pass through an 80-mesh sieve to obtain a mixture.

[0059] The iron powder is 100% FHY80.25 reduced iron powder produced by Luyin New Materials, with a bulk density of 2.52 g / cm 3 , flow rate 30S / 50g, compressibility ≥6.55g / cm 3 (490MPa).

[0060] The zinc stearate has a melting point of 122°C.

[0061] The graphite has a model number of LC-325-999.

[0062] The cutting agent is MnS cutting agent.

[0063] In the batching step, the weight percentage of each raw material is as follows: 0.8% zinc stearate, 0.85% graphite, 0.55% cutting agent, and the balance is reduced iron powder.

[0064] 2. Suppression

[0065] The mixed material is put into a molding machine, the pressing density is controlled at 6.3 g / cm3, and the mixed material is pressed to obtain a blank.

[0066] During the pressing process, the mold is fully demagnetized; and the density uniformity of the blank is not greater than 0.1g / cm 3 .

[0067] 3. Sintering

[0068] The blank is placed on a flat plate in the sintering furnace for sintering. The number of layers of the product is determined according to the height of the furnace. During the sintering process, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas. The blank is first sintered and dewaxed at 685℃ for 45 minutes; then sintered at 985℃ for 45 minutes; after sintering, the blank is cooled to 105℃ and taken out of the furnace, immersed in treatment oil for 15 minutes to obtain a sintered part.

[0069] Among them, the volume ratio of hydrogen to ammonia decomposition gas is 1:9.5.

[0070] The treatment oil is composed of 32# machine oil and F5-1 anti-rust oil, and the weight ratio of 32# machine oil to F5-1 anti-rust oil is 6:5.

[0071] 4. Machining

[0072] The cutting piece is obtained by cutting the sintered part using a cubic boron nitride machining blade.

[0073] 5. Post-processing

[0074] The cutting parts were subjected to oil quenching treatment for 35 minutes and then polishing treatment for 45 minutes to obtain powder metallurgy steel collars.

[0075] Wherein, the temperature of the oil quenching treatment is 845°C.

[0076] The powder metallurgy steel collar has a surface hardness of HRA62, an oil content of more than 15.5%, and a porosity of 22%.

[0077] Example 3

[0078] A method for producing a powder metallurgy steel collar is as follows:

[0079] 1. Ingredients

[0080] Take 60% of the total amount of iron powder, mix it with zinc stearate, graphite and cutting agent, and mix them evenly; add the remaining amount of iron powder and continue mixing for 50 minutes. After mixing for 30 minutes, pass it through an 80-mesh sieve to obtain a mixture.

[0081] The iron powder is 100% FHY80.25 reduced iron powder produced by Luyin New Materials, with a bulk density of 2.52 g / cm 3 , flow rate 30S / 50g, compressibility ≥6.55g / cm 3 (490MPa).

[0082] The zinc stearate has a melting point of 122°C.

[0083] The graphite has a model number of LC-325-999.

[0084] The cutting agent is MnS cutting agent.

[0085] In the batching step, the weight percentage of each raw material is as follows: 0.85% zinc stearate, 0.9% graphite, 0.6% cutting agent, and the balance is reduced iron powder.

[0086] 2. Suppression

[0087] The mixture was put into a molding machine and the compaction density was controlled at 6.4 g / cm 3 , pressed into shape, to obtain a blank.

[0088] During the pressing process, the mold is fully demagnetized; and the density uniformity of the blank is not greater than 0.1g / cm 3 .

[0089] 3. Sintering

[0090] The blank is placed on a flat plate in the sintering furnace for sintering. The number of layers of the product is determined according to the height of the furnace. During the sintering process, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas. The blank is first sintered and dewaxed at 690°C for 50 minutes; then sintered at 990°C for 50 minutes; after sintering, the blank is cooled to 110°C and taken out of the furnace, immersed in treatment oil for 20 minutes to obtain a sintered part.

[0091] The volume ratio of hydrogen to ammonia decomposition gas is 1:10.

[0092] The treatment oil is composed of 32# machine oil and F5-1 anti-rust oil, and the weight ratio of 32# machine oil to F5-1 anti-rust oil is 6:6.

[0093] 4. Machining

[0094] The cutting piece is obtained by cutting the sintered part using a cubic boron nitride machining blade.

[0095] 5. Post-processing

[0096] The cutting parts were subjected to oil quenching treatment for 40 minutes and then polishing treatment for 50 minutes to obtain powder metallurgy steel collars.

[0097] Wherein, the temperature of the oil quenching treatment is 850°C.

[0098] The powder metallurgy steel collar has a surface hardness of HRA60, an oil content of more than 15.1%, and a porosity of 20%.

[0099] Example 4

[0100] A method for producing a powder metallurgy steel collar is as follows:

[0101] 1. Ingredients

[0102] Take 50% of the total amount of iron powder and mix it with modified alumina powder, zinc stearate, graphite, hydroxypropyl methylcellulose and cutting agent. After mixing evenly, add the remaining amount of iron powder and continue mixing for 40 minutes. After 20 minutes of batching, pass through an 80-mesh sieve; then use a 60Co source to control the radiation dose to 200KGy for radiation treatment, and obtain a mixture after the radiation is completed.

[0103] In the batching step, the weight percentage of each raw material is as follows: 3% modified alumina powder, 0.75% zinc stearate, 0.8% graphite, 0.9% hydroxypropyl methylcellulose, 0.5% cutting agent, and the balance is reduced iron powder.

[0104] The iron powder is 100% FHY80.25 reduced iron powder produced by Luyin New Materials, with a bulk density of 2.52 g / cm 3 , flow rate 30S / 50g, compressibility ≥6.55g / cm 3 (490MPa).

[0105] The zinc stearate has a melting point of 122°C.

[0106] The graphite has a model number of LC-325-999.

[0107] The cutting agent is MnS cutting agent.

[0108] The modified alumina powder is prepared by the following method: adding alumina powder with a particle size of 2 μm into a 2-fold volume of a treatment liquid, stirring at 200 rpm for 2 hours at a temperature of 55° C.; then placing the powder in a vacuum environment of 0.05 MPa at a temperature of 65° C. and keeping the temperature until no solvent gas is distilled out; grinding at a grinding speed of 2500 rpm to a particle size of 100 nm to obtain the modified alumina powder.

[0109] The preparation method of the treatment liquid is as follows: grind polycarbosilane into powder, add the powder into n-hexane, adjust the volume concentration of polycarbosilane in n-hexane to 50%, heat it to 60°C at a heating rate of 0.2°C / min, stir at 60rpm for 4h, and prepare the treatment liquid.

[0110] 2. Suppression

[0111] The mixture was put into a molding machine and the compaction density was controlled at 6.2 g / cm 3, pressed into shape, to obtain a blank.

[0112] During the pressing process, the mold is fully demagnetized; and the density uniformity of the blank is not greater than 0.1g / cm3.

[0113] 3. Sintering

[0114] The blank is placed on a flat plate in the sintering furnace for sintering, and the number of layers of the product is determined according to the height of the furnace. During the sintering process, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas. The blank is first sintered and dewaxed at 680°C for 40 minutes; then sintered at 1050°C for 40 minutes; after sintering, the blank is cooled to 100°C and taken out of the furnace, immersed in treatment oil for 10 minutes to obtain a sintered part.

[0115] The volume ratio of hydrogen to ammonia decomposition gas is 1:9.

[0116] The treatment oil is composed of 32# machine oil and F5-1 anti-rust oil, and the weight ratio of 32# machine oil to F5-1 anti-rust oil is 6:4.

[0117] 4. Machining

[0118] The cutting piece is obtained by cutting the sintered part using a cubic boron nitride machining blade.

[0119] 5. Post-processing

[0120] The cutting parts were subjected to oil quenching treatment for 30 minutes and then polishing treatment for 40 minutes to obtain powder metallurgy steel collars.

[0121] Wherein, the temperature of the oil quenching treatment is 840°C.

[0122] The powder metallurgy steel collar has a surface hardness of HRA68, an oil content of 16.9%, and a porosity of 29%.

[0123] Unless otherwise specified, all percentages used in the present invention are by mass.

[0124] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for producing a powder metallurgy steel collar, characterized in that: The production method includes: batching, pressing, sintering, machining, and post-processing; The ingredients are as follows: 50% of the total amount of iron powder is taken and mixed with modified alumina powder, zinc stearate, graphite, hydroxypropyl methylcellulose and cutting agent, and the mixture is uniformly mixed; the remaining amount of iron powder is added and the mixing is continued for 40 minutes, and after 20 minutes of batching, the mixture is passed through an 80-mesh sieve; then a 60Co source is used to control the radiation dose to 200KGy for radiation treatment, and a mixture is obtained after the radiation is completed; In the batching step, the weight percentage of each raw material is as follows: 3% modified alumina powder, 0.75% zinc stearate, 0.8% graphite, 0.9% hydroxypropyl methylcellulose, 0.5% cutting agent, and the balance is reduced iron powder; The iron powder is 100% FHY80.25 reduced iron powder produced by Luyin New Materials, with a bulk density of 2.52 g / cm 3 , flow rate 30S / 50g, compressibility at 490MPa ≥6.55g / cm 3 ; The zinc stearate has a melting point of 122°C; The graphite model is LC-325-999; The cutting agent is a MnS cutting agent; The modified alumina powder is prepared by the following method: adding alumina powder with a particle size of 2 μm into a treatment liquid with a volume of 2 times, stirring at 200 rpm for 2 hours at a temperature of 55° C.; then placing it in a vacuum environment with a degree of vacuum of 0.05 MPa and a temperature of 65° C., and keeping it warm until no solvent gas is distilled out; grinding at a grinding speed of 2500 rpm to a particle size of 100 nm, thereby preparing the modified alumina powder; The preparation method of the treatment liquid is as follows: grind polycarbosilane into powder, add the powder into n-hexane, adjust the volume concentration of polycarbosilane in n-hexane to 50%, heat it to 60°C at a heating rate of 0.2°C / min, stir at 60rpm for 4h, and prepare the treatment liquid; The mixture is pressed into a shape to obtain a blank, and the pressing density is controlled at 6.2 g / cm 3 ; In the pressing step, the mold is fully demagnetized; and the density uniformity of the blank is not greater than 0.1g / cm 3 ; During the sintering process, the sintering atmosphere is a mixed atmosphere of hydrogen and ammonia decomposition gas; the blank is first sintered and dewaxed at 680°C for 40 minutes; then sintered at 1050°C for 40 minutes; after the sintering is completed, the blank is cooled to 100°C and taken out of the furnace, and immersed in treatment oil for 10 minutes to obtain a sintered part; In the sintering step, the volume ratio of hydrogen to ammonia decomposition gas is 1:9; The treatment oil is composed of 32# machine oil and F5-1 anti-rust oil, and the weight ratio of 32# machine oil to F5-1 anti-rust oil is 6:4; The machining comprises cutting the sintered part to obtain a cutting part; The post-treatment is to perform oil quenching treatment on the cutting piece for 30 minutes and then perform finishing treatment for 40 minutes to obtain a powder metallurgy steel collar; The temperature of the oil quenching treatment is 840°C.

Citation Information

Patent Citations

  • Preparation method for powder metallurgical steel collar ring of ring-twisting frame

    CN103317134A

  • Sintered Ring Composition for Spinning and Twisting, Sintered Ring containg the composition and manufacturing mehtod thereof

    KR102158336B1