A production method for extra-thick modular steel for cold working dies
By isothermal spherical annealing, milling and single-filament gas-electric vertical welding of continuous casting billets of cold-work mold steel, combined with forging and differential temperature rolling, the composition segregation and welding crack problems in the production of extra-thick mold steel are solved. , realizes the production of extra-thick modules with high material yield and dimensional accuracy.
Patent Information
- Application Number
- CN202310169016.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The existing technology is difficult to effectively produce cold-work mold steel with extra-thick specifications of more than 200mm. The mold casting process leads to serious segregation of components, long production cycle, low material yield, and high welding crack sensitivity of high carbon mold steel, which cannot meet the composite extra-thick module. production demand.
Isothermal spherical annealing was used for continuous casting, and after milling and grinding, the blank was then soldered through a single-filament gas-electric vertical welding group. Combined with forging and differential temperature rolling, AWS A5.26 EG70T-2 welding wire and CO2 gas were used for reserved welding. Seam pumping and spot welding sealing, followed by cooling and heat treatment to ensure the bonding strength of the composite interface.
The high material yield, dimensional accuracy and internal tissue density of 200-400mm thick cold work mold steel is achieved, and the composite bonding degree is as high as 96.5%. The shear strength and impact toughness meet the standard requirements, reducing production costs.
Smart Images

Figure CN116175098B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material processing, and in particular relates to a production method of extra-thick modular steel for cold working dies. Background Art
[0002] Cold working die steel has good toughness, wear resistance and hardenability, and is widely used in the manufacture of various cold working dies with complex structures and heavy working conditions. The development trend of large-scale and efficient mold industry has a strong demand for large modules with extra-thick specifications of more than 200mm. At present, the large modules for producing cold working dies with extra-thick specifications of more than 200mm are usually obtained by die casting to ensure the compression ratio. However, the inherent defects of the die casting process lead to a series of problems, such as serious segregation of ingot composition, long casting process time, high energy consumption, and certain pollution to the environment. At the same time, the rolling rate of die-cast steel ingots is low and the product development cost is high.
[0003] Vacuum composite rolling technology is an effective method for producing extra-thick steel plates, which solves the problem of limited thickness of extra-thick steel plates due to the thickness and compression ratio of continuous casting billets. Compared with the traditional die casting process, vacuum composite rolling products have better internal structure and performance, and a high yield rate. At present, some domestic steel mills have been able to produce high-quality ordinary carbon low-alloy steel extra-thick steel plates through vacuum composite rolling technology. However, for Cr12MoV and other Cr12MoV type die steel varieties with high carbon and alloy content, due to the high sensitivity of weld cracks, welding and post-weld cooling processes are very likely to cause weld cracking and even cracking of the base billet, and the production of composite extra-thick modules cannot be completed. In addition, the thermal stress of cold working die steel in the subsequent fire cutting and heat treatment process is greater than that of general die steel varieties such as hot working and corrosion resistant, and the composite interface bonding strength requirements are higher. Conventional composite rolling processes are difficult to meet the requirements. There is no relevant research on cold working die steel composite billets in China.
[0004] Publication No. CN110195186A discloses “an extra-thick hot-rolled high-alloy hot working die steel and a preparation method thereof”, which only solves the production problem of extra-thick die steel plates with an alloy (Cr+Mn+Ni+Cu) content of ≤3.7%.
[0005] Publication number CN101773931A discloses "a method for vacuum composite rolling of extra-thick plates", publication number CN103692166A "a method for preparing extra-thick alloy steel plates", CN101590596B "a method for manufacturing extra-thick slabs by cumulative lap welding process", publication number CN103028897 A "a method for producing extra-thick steel plates with high cold crack sensitivity", and publication number CN105252237A "a method for producing CrMnNiMo-based extra-thick mold composite billets", etc. All of them use vacuum electron beam welding technology to weld and assemble continuous casting billets to solve the production problem of high-alloy extra-thick steel plates. However, this process requires welding operations to be performed in a closed vacuum chamber, and the weld state cannot be grasped in real time. The weld can only be observed after the welding is completed and the air is broken. For high-carbon mold steel varieties, the welding crack sensitivity is high, and cracking is very likely to occur during the welding process. Vacuum electron beam welding cannot achieve timely repair welding, resulting in a decrease in the success rate of billet assembly. Summary of the invention
[0006] The present invention provides a method for producing extra-thick modular steel for cold working dies, which adopts continuous casting billets as basic raw materials to produce extra-thick modular steel for cold working dies with a thickness of 200-400 mm and high flaw detection and composite interface bonding strength. The present invention has low cost, high yield rate, high dimensional accuracy and strong operability.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for producing extra-thick modular steel for cold working dies, comprising:
[0009] 1) Billet annealing:
[0010] The continuous casting billet is subjected to isothermal spheroidizing annealing treatment to obtain uniform and fine spheroidized pearlite structure, which is convenient for billet assembly welding. The heating temperature is 860-880℃, and the temperature is kept for 6-8h. Then the furnace is cooled to 740-760℃, and the temperature is kept for 8-12h. Then the furnace is cooled to ≤600℃ and taken out of the furnace.
[0011] 2) Billet processing:
[0012] The surface of the continuous casting billet to be composited is milled and ground to remove the oxide layer and rust layer to prevent the diffusion and bonding of the matrix from being hindered during the subsequent heating and rolling process; in the above step 2), after the milling and grinding, the gap between the continuous casting billets is ≤2mm, and the surface roughness Ra is ≤50μm; the length and width of a group of billets to be composited differ by ≤10mm; then the four sides of the surface to be composited are chamfered, and the chamfering size is (15-20mm)×(40-50)°;
[0013] 3) Welding:
[0014] The welding adopts the single-wire gas-electric vertical welding method, and the billet is welded along the four sides of the billet. In order to ensure the strength of the weld and combine the characteristics of the steel composition, the welding wire is selected as the brand AWS A5.26 EG70T-2 flux-cored welding wire, the wire speed is 5-8m / min, the CO2 gas flow is 24-32L / min, the cooling water flow is 1.0-1.5L / min, the welding current is 140-160A, the arc voltage is 26-30V, the welding speed is 8-10cm / min, and the weld exhaust hole is reserved. Then a vacuum pump is used to extract the vacuum from the weld exhaust hole to a vacuum degree of ≤1Pa, and then spot welding is used to complete the sealing;
[0015] 4) Slow cooling after welding:
[0016] After welding is completed, the composite billet is sent to the slow cooling pit for insulation to reduce the sensitivity of welding cracks and eliminate welding stress. The heating temperature is 200-300℃. After insulation for 2-3 hours, it is cooled with the furnace. After that, the composite billet is hoisted to the heating furnace for heating;
[0017] 5) Heating:
[0018] Heating temperature 1140~1180℃, heating time 1.5~2h / 100mm thickness;
[0019] 6) Forging intermediate billet:
[0020] A 3000-ton hydraulic press is used to forge the composite billet. The forging direction is perpendicular to the composite interface. The initial forging temperature is ≥1000℃, the final forging temperature is ≥850℃, the material is forged in one fire, and the total forging ratio is 1.5. After forging, it is slowly cooled to room temperature in a slow cooling pit to reduce thermal stress and structural stress.
[0021] 7) Intermediate billet heating:
[0022] Before loading into the furnace, add "cold rolled plate" on the surface of the intermediate billet with a thickness of 0.8-1.2mm; heat preservation at 700-750℃ for 5-7h, heating time at 700-1220℃ for 4-6h, and heat preservation at 1180-1220℃ for 5-7h. The total time in the furnace is ≤22h;
[0023] 8) Composite billet rolling:
[0024] The first two passes of rolling are empty and the rack descaling water is turned on for descaling to ensure that the cold-rolled plate on the upper surface of the billet is cleaned; the surface of the intermediate billet is quickly cooled by the instant cooling device between passes, and rolling is started when the surface is cooled to between 650 and 720°C; the surface of the billet is cooled and controlled by the instant cooling device between passes for rolling 2 to 4 passes, the target cooling temperature is 600 to 650°C, the roller speed is 0.8 to 1.2 m / s, and the reduction of each pass in the first 4 passes is not less than 30 mm;
[0025] 9) Heat treatment:
[0026] Tempering, tempering temperature 260℃~350℃, holding time 12~16h.
[0027] In order to ensure the internal quality, the continuous casting billets which are more than 3m away from the head and tail of the continuous casting billets are selected as the billets to be composited. After the continuous casting billets are off the line, they are stacked and slowly cooled for no less than 48 hours.
[0028] The chemical composition of the extra thick module steel for cold working die is calculated by weight as follows: C 1.30%~1.75%, Si0.3~0.8%, Mn 0.3~1.0%, Cr 10.0%~13.0%, Mo 0.3%~1.4%, V 0.1%~0.5%, P≤0.030%, S≤0.020%, and the rest is Fe and unavoidable impurities.
[0029] The finished thickness of the extra thick modular steel for cold working dies is 200 to 400 mm.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention provides a method for producing extra-thick modules for cold-working die steel varieties mainly based on Cr12MoV, which have problems such as long die casting production cycle, low yield rate, poor homogeneity of extra-thick specification modules, severe segregation leading to poor quality, and composite welding cracking and insufficient composite surface bonding strength due to the characteristics of the steel type, and effectively solves the production problem of extra-thick composite modules of cold-working die steel. The present invention uses gas-electric vertical welding to assemble continuous casting billets, and produces extra-thick modules by combining forging + differential temperature rolling, which improves the internal organization density of the billet, ensures the interface bonding strength, and meets the dimensional accuracy requirements of cold-working die steel. The composite modules with a thickness of 200-400 mm produced by the present invention have an ultrasonic flaw detection reaching the GB / T64023 level, a composite bonding degree of more than 96.5%, a shear strength far exceeding the requirements of GB / T 8165, and impact toughness and hardness both meet the requirements of SAE standards. The present invention realizes the production of extra-thick modules of cold-working die steel using continuous casting billets as raw materials. Compared with technologies such as die casting and electroslag remelting, the present invention has the advantages of high yield rate and good internal quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the core structure (composite interface) of the 350mm extra-thick composite module of the present invention.
[0033] Figure 2 This is the 350mm extra-thick composite module matrix structure of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0035] The chemical composition of the steel grades of the embodiments of the present invention is shown in Table 1, the annealing and processing parameters of the continuous casting billet of the embodiments are shown in Tables 2 and 3, the welding assembly process parameters of the embodiments are shown in Table 4, the forging process of the intermediate billet of the embodiments is shown in Table 5, the rolling process of the embodiments is shown in Table 6, the heat treatment process of the embodiments is shown in Table 7, and the actual effect is shown in Table 8.
[0036] Table 1 Chemical composition of steel smelting in each example (%)
[0037] Example C Si Mn P S Cr Mo V 1 1.30 0.6 0.6 0.020 0.008 12.6 1.2 0.5 2 1.75 0.5 0.3 0.016 0.010 10.0 0.9 0.2 3 1.58 0.8 1.0 0.010 0.005 11.5 1.4 0.4 4 1.46 0.3 0.8 0.012 0.015 13.0 0.3 0.1 5 1.35 0.6 0.6 0.010 0.005 12.5 0.6 0.2
[0038] Table 2 Annealing process parameters of continuous casting billets in various embodiments
[0039]
[0040] Table 3 Processing parameters of continuous casting billets in various embodiments
[0041]
[0042]
[0043] Table 4 Process parameters of welding assembly in various embodiments
[0044]
[0045] Table 5 Forging process parameters of intermediate billet in each embodiment
[0046]
[0047] Table 6 Process parameters for heating and rolling of intermediate billets in various embodiments
[0048]
[0049] Table 7 Heat treatment process of each embodiment
[0050] Example Finished product thickness / mm Tempering temperature / ℃ Insulation time / h 1 200 260 16 2 400 350 12 3 260 300 16 4 240 300 14 5 350 320 15
[0051] Table 8 Actual effects of various embodiments
[0052]
[0053] Figure 1 and Figure 2 It is the metallographic structure diagram of Example 5, from Figure 1 It can be seen that no obvious dividing line is found in the composite interface of the extra-thick module of the present invention, and the composite interface achieves good metallurgical bonding.
Claims
1. A method for producing extra thick modular steel for cold working dies, characterized in that the method include: 1) Billet annealing: The continuous casting billet is subjected to isothermal spheroidizing annealing treatment, with a heating temperature of 860-880°C, kept at this temperature for 6-8h, then cooled in the furnace to 740-760°C, kept at this temperature for 8-12h, and then cooled in the furnace to ≤600°C before being taken out of the furnace; 2) Welding: The welding adopts the single-wire gas-electric vertical welding method, and the welding is carried out along the welding grooves on the four sides of the billet. The wire speed is 5-8m / min, the CO2 gas flow rate is 24-32L / min, the cooling water flow rate is 1.0-1.5L / min, the welding current is 140-160A, the arc voltage is 26-30V, the welding speed is 8-10cm / min, and the weld exhaust hole is reserved. Then a vacuum pump is used to extract the vacuum from the weld exhaust hole to a vacuum degree of ≤1Pa, and then spot welding is used to complete the sealing; 3) Slow cooling after welding: After welding is completed, the composite billet is sent to the slow cooling pit for insulation and then slow cooling. The heating temperature is 200-300°C. After insulation for 2-3 hours, it is cooled with the furnace. After that, the composite billet is hoisted to the heating furnace for heating. 4) Heating: Heating temperature is 1140~1180℃, heating time is 1.5~2h / 100mm thickness; 5) Forging intermediate billet: The forging direction is perpendicular to the composite interface, the initial forging temperature is ≥1000℃, the final forging temperature is ≥850℃, the material is forged in one fire, and after forging, it is slowly cooled to room temperature in a slow cooling pit; 6) Intermediate billet heating: Before loading into the furnace, cover the surface of the intermediate billet with "cold rolled plate" with a thickness of 0.8-1.2mm; heat preservation at 700-750℃ for 5-7h, heating time at 700-1220℃ for 4-6h, and heat preservation at 1180-1220℃ for 5-7h. The total time in the furnace is ≤22h; 7) Composite billet rolling: The surface of the intermediate billet is rapidly cooled, and rolling is started when the surface cools to between 650 and 720°C; the billet surface is cooled and temperature controlled for 2 to 4 passes, the target cooling temperature is 600 to 650°C, the roller speed is 0.8 to 1.2 m / s, and the reduction in each of the first 4 passes is not less than 30 mm; 8) Heat treatment: Tempering, tempering temperature 260℃~350℃, holding time 12~16h; The chemical composition of the steel is calculated by weight percentage: C 1.30%~1.75%, Si≤0.8%, Mn≤1.0%, Cr 10.0%~13.0%, Mo 0.3%~1.4%, V 0.1%~0.5%, P≤0.030%, S≤0.020%, and the rest is Fe and unavoidable impurities; The finished thickness of the extra thick modular steel for cold working dies is 200 to 400 mm.
2. The method for producing extra thick modular steel for cold working dies according to claim 1, characterized in that: After the billet is annealed, the surface to be composited of the continuous casting billet is milled and ground to remove the oxide layer and the rust layer. After the milling and grinding, the gap between the continuous casting billets is ≤2mm and the surface roughness Ra is ≤50μm.
3. The method for producing extra thick modular steel for cold working dies according to claim 1, characterized in that: In the above step 7), the first two rolling passes are passed without any scale removal water and the stand is turned on for descaling.
4. The method for producing extra thick modular steel for cold working dies according to claim 1, characterized in that: Select the continuous casting billets that are more than 3m away from the head and tail of the continuous casting billet as the billets to be composited. After the continuous casting billets come off the line, they shall be stacked and slowly cooled for no less than 48 hours.
Citation Information
Patent Citations
Method for manufacturing extra-thick plate blank by accumulative roller welding process
CN101590596B
Method for rolling special thick board by means of vacuum compositing
CN101773931A
Manufacture method for cold-crack and high sensibility ultra-thick steel plate
CN103028897A
Preparation method of super-thick alloy steel plate
CN103692166A
Method for producing CrMnNiMo series ultra-thick mold compound billets
CN105252237A