A production method for extra-thick modular steel for corrosion-resistant molds

By milling and preheating the continuous casting billet, combined with single-wire gas-electric vertical welding and vacuum pump technology, two-fire heating forging and water mist-air alternating controlled quenching were performed to solve the welding cracking of high-alloy corrosion-resistant mold steel. In order to solve the problem of low interface bonding strength, it has achieved efficient and low-cost production of extra-thick module steel, meeting the needs of corrosion-resistant molds with a thickness of 300-600mm.

CN116175099BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310169022.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-10-22
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

It is difficult to effectively produce extra-thick martensitic stainless steel for high-alloy corrosion-resistant molds with existing technology, especially SUS420, S136 and other varieties. Due to the high sensitivity of welding cracks, the welding process can easily cause cracking, and the bonding strength of the composite surface is low, which reduces production efficiency. Low and poor quality.

Method used

Based on the continuous casting billet, the oxide layer is removed by milling, preheating is used to reduce the welding heat affected zone, single wire gas and electric vertical welding technology is used for welding, combined with vacuum pump extraction and spot welding sealing, and two-fire heating and forging is performed. The water mist-air alternating time-controlled quenching + tempering process is used to ensure the strength of the weld and the bonding of the interface.

Benefits of technology

It has achieved low-cost and high-efficiency production of 300-600mm thick extra-thick modular steel with high homogeneity and high interface bonding strength. The yield rate is high, the composite interface bonding degree reaches more than 92%, and the shear strength and corrosion resistance meet the standards. , suitable for corrosion-resistant molds with a thickness of 200~600mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116175099B_ABST
    Figure CN116175099B_ABST
Patent Text Reader

Abstract

The present invention relates to a production method of extra-thick module steel for corrosion-resistant molds. The composite blank is preheated before welding; welding is performed by single-wire gas-electric vertical welding; heating after welding: two-fire heating is performed before forging; the composite blank is forged by free forging; and heat treatment is performed by water mist-air alternating time-controlled quenching + tempering process. The present invention has a high yield rate and lower production cost than processes such as die casting and electroslag remelting. The composite module with a thickness of 200-600mm produced by the present invention has a composite interface bonding degree of more than 92%, a shear strength that meets the requirements of GB / T 8165, an ultrasonic flaw detection that reaches GB / T6402 Level 4, and a corrosion weight loss rate of less than 0.5g / m in a 3.5% NaCl salt spray environment. 2 h, the polishing grade reaches PLASTICS A2 standard, and the production of extra-thick modules for 300-600mm corrosion-resistant molds is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material processing, and in particular relates to a production method of extra-thick module steel for corrosion-resistant moulds. Background Art

[0002] The injection molding industry is developing rapidly towards diversification, complexity and high precision. Corrosive polymer materials such as polyvinyl chloride, polypropylene, ABS, EVA, polyurethane, etc. are widely used, which puts higher requirements on the corrosion resistance of injection molds. Corrosion-resistant mold steel is a special steel type for molds that has emerged in response to the development of the industry. With the widespread application of CAD / CAM / CAE integrated technology, trends such as one mold with multiple cavities and large-scale molds have put forward higher requirements on the thickness specifications of corrosion-resistant mold steel.

[0003] Limited by the thickness specifications of continuous casting billets, the current production of extra-thick corrosion-resistant and extra-thick modules usually adopts die casting and electroslag remelting. Using die casting to obtain large-sized steel ingots and produce extra-thick steel plates can ensure a certain compression ratio, but the inherent defects of the die casting process lead to a series of problems, such as serious segregation of ingot components, long casting process time, high energy consumption, certain pollution to the environment, and low rolling yield, generally not exceeding 70%, and poor economic efficiency; electroslag remelting can obtain an internal structure with higher cleanliness, and at the same time can reduce the segregation problem of steel billets, and then electroslag remelting requires the steel billets to be melted twice, which is inefficient, consumes a lot of energy, and the production cost is too high.

[0004] Vacuum composite rolling technology is an effective method for producing extra-thick steel plates, which solves the problem of limited thickness of extra-thick steel plates due to the thickness and compression ratio of continuous casting billets. Compared with the traditional die casting process, vacuum composite rolling products have better internal structure and performance, and a high yield rate. Compared with electroslag remelting, it has high production efficiency and low cost, which is conducive to organizing mass production. At present, some domestic steel mills have been able to produce high-quality ordinary carbon low-alloy steel extra-thick steel plates through vacuum composite rolling technology. However, for martensitic stainless steels for molds with high C and Cr contents such as SUS420 and S136, due to the high sensitivity of weld cracks, weld cracking is very likely to occur during welding and post-weld cooling, and even cause cracking of the base billet, making it impossible to complete the production of composite extra-thick modules, and related successful cases are rarely reported.

[0005] Publication No. CN110195186A discloses “an extra-thick hot-rolled high-alloy hot working die steel and a preparation method thereof”, which only solves the production problem of extra-thick die steel plates with an alloy (Cr+Mn+Ni+Cu) content of ≤3.7%.

[0006] Publication number CN101773931A discloses "a method for vacuum composite rolling of extra-thick plates", publication number CN103692166A "a method for preparing extra-thick alloy steel plates", CN101590596B "a method for manufacturing extra-thick slabs by cumulative lap welding process", publication number CN103028897 A "a method for producing extra-thick steel plates with high cold crack sensitivity", and publication number CN105252237A "a method for producing CrMnNiMo-based extra-thick mold composite billets", etc. All of them use vacuum electron beam welding technology to weld and assemble continuous casting billets to solve the production problem of high-alloy extra-thick steel plates. However, this process requires welding operations to be performed in a closed vacuum chamber, and the weld state cannot be grasped in real time. The weld can only be observed after the welding is completed and the air is broken. For high-alloy mold steel varieties, the welding crack sensitivity is high, and cracking is very likely to occur during the welding process. Vacuum electron beam welding cannot achieve timely repair welding, resulting in a decrease in the success rate of assembly. In addition, there is also the problem of low bonding strength of the composite surface, which leads to problems such as delamination and cracking of the composite surface during subsequent heat treatment, processing and use. Summary of the invention

[0007] The present invention provides a method for producing extra-thick module steel for corrosion-resistant molds, which adopts continuous casting billets as basic raw materials to produce extra-thick modules for corrosion-resistant molds with a thickness of 300-600mm and excellent flaw detection and performance. The present invention has low cost, high yield rate and strong operability.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for producing extra-thick module steel for corrosion-resistant molds, comprising:

[0010] 1) Composite billet processing:

[0011] The surface of the continuous casting billet to be composited after slow cooling and unstacking is milled and ground to remove the oxide layer and rust layer to prevent the diffusion and bonding of the matrix from being hindered during the subsequent heating and rolling process; after milling and grinding, the gap between the continuous casting billets is ≤2mm and the surface roughness Ra is ≤50μm;

[0012] The length and width of a group of blanks to be composited differ by ≤10mm; then the four sides of the composite surface are chamfered, with the chamfer size of (15~20mm)×(40~50)°

[0013] 2) Preheating of composite billet before welding:

[0014] Align the surfaces of the processed continuous casting billets to be composited, stack them up and down, and use electric heating asbestos pads to cover the billets along the chamfered positions around the billets and preheat them to reduce the temperature difference in the welding heat affected zone and avoid weld cracking. The preheating temperature is 200-300℃ and the preheating time is 3-4h. The electric heating asbestos pad can not only realize the preheating function of the area near the chamfer, but also prevent the surface of the billet to be composited from being oxidized due to high temperature, which affects the composite effect.

[0015] 3) Welding:

[0016] The welding adopts the single-wire gas-electric vertical welding method, and the billet is welded along the four sides. In order to ensure the strength of the weld and combine the characteristics of the steel composition, the welding wire is the AWS A5.22 E316LT1-1 flux-cored wire, the wire speed is 10-15m / min, CO 2 Gas flow rate is 20-30L / min, cooling water flow rate is ≥2L / min, welding current is 280-380A, arc voltage is 34-40V, welding speed is 15-25cm / min, weld seam exhaust holes are reserved, vacuum is then extracted from the weld seam exhaust holes using a vacuum pump until the vacuum degree is ≤1Pa, and then spot welding is used to complete the sealing;

[0017] 4) Post-weld heating:

[0018] After welding is completed, the weld area is again coated and heated with an electric heating asbestos pad to promote the escape of hydrogen in the weld, prevent delayed cracking, and reduce welding residual stress. The heating temperature is 150-200°C and the holding time is 4-5 hours. After that, the composite billet is hoisted to the heating furnace for heating;

[0019] 5) Heating forging:

[0020] Two-fire heating forging is adopted, with the target heating temperature of 1200℃~1240℃, the heating time of the first fire is 1.5~2h / 100mm thickness, and the second fire is heated to the target heating temperature and the holding time is 2.5~4h to ensure that the composite billet is evenly burned through and avoid coarse grains caused by too long heating time;

[0021] After the billet is taken out of the furnace, water mist is used to cool its upper surface. The water temperature of the water mist is ≤35℃, the volume ratio of water to air in the water mist is 1:180~1:220, and the cooling temperature is 800~850℃, so that a layer of "low-temperature hard shell" is formed on the surface, thereby enhancing the penetration of the forging force into the core of the billet during the forging process; a 3000-ton hydraulic press is used to forge the composite billet, and the upper and lower hammers are of asymmetric size to further improve the forging permeability of the billet and strengthen the bonding degree of the composite interface; the upper hammer is of width W=0.4~0.5H and length L =1.5~1.8W′ flat hammer head, the width of the lower forging platform is ≥2.0W′, H and W′ are the height and width of the composite blank respectively, the length direction of the upper hammer head is perpendicular to the width direction of the lower platform and the feeding direction of the blank, and the forging direction is perpendicular to the composite interface of the blank; the initial forging temperature (1 / 2 of the blank thickness) is ≥1150℃, the final forging temperature (1 / 2 of the blank thickness) is ≥800℃, the material is forged in two fires, the total forging ratio is 1.5~2, the single-pass forging feed is 0.8~1.0W, and it is air-cooled to room temperature after forging;

[0022] 6) Heat treatment:

[0023] The heat treatment adopts water mist-air alternating time-controlled quenching + tempering process, which can not only ensure that the core of the thick module is quenched martensite, but also prevent the surface quenching stress from being too large and cracking. The water temperature is ≤35℃, and the volume ratio of water to air in the water mist is 1:450~1:470. The water mist-air alternating time-controlled quenching process is: heating temperature 1000~1050℃, net holding time 1~1.4min / mm thickness, then air cooling for 15~25min → water mist cooling for 20~40min → air cooling for 50~70min, water mist cooling for 1.5~3h → air cooling to room temperature, tempering temperature 610℃~640℃, holding time 3~4min / mm thickness.

[0024] To ensure the internal quality, the continuous casting billets more than 3m away from the head and tail of the continuous casting billet are selected as the billets to be composited. After the continuous casting billets are off the line, they are stacked and slowly cooled to reduce the hardness of the billets and improve the subsequent surface milling efficiency. The stacking temperature is ≥650℃ and the stacking time is ≥48h.

[0025] A special thick module steel for corrosion-resistant molds, wherein the chemical composition of the steel is as follows by weight: C 0.20%-0.45%, Si 0.30%-1.0%, Mn 0.30%-1.0%, Cr 10.5%-18.0%, Ni≤1.20%, Mo≤1.2%, V≤0.50%, P≤0.040%, S≤0.050%, and the rest is Fe and unavoidable impurities.

[0026] The finished thickness of the extra-thick modular steel for corrosion-resistant molds is 300 to 600 mm.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention provides a method for producing extra-thick modules at low cost and high efficiency for corrosion-resistant mold steel varieties mainly based on Cr-based martensitic stainless steel, which have problems such as long die casting production cycle, low yield rate, poor homogeneity of extra-thick specification modules, severe segregation leading to poor quality, and welding cracking and low composite interface bonding strength caused by the characteristics of the steel type, and effectively solves the production problem of extra-thick martensitic stainless steel composite modules for Cr-based corrosion-resistant molds. The present invention uses continuous casting billets as raw materials, and the internal quality is better than that of die-cast steel ingots. It adopts gas-electric vertical welding technology for billet assembly welding to ensure the quality of the weld and improve welding efficiency. It combines a 1.5-2 times low forging ratio, asymmetric deformation, and high interface permeability forging composite process to achieve the production of composite modules with high homogeneity and high interface bonding strength under low compression ratio conditions. The invention has a high yield rate and a production cost lower than that of die casting, electroslag remelting and other processes. The composite module with a thickness of 300-600 mm produced by the invention has a composite interface bonding degree of more than 92%, a shear strength that meets the requirements of GB / T 8165, an ultrasonic flaw detection that reaches GB / T6402 level 4, and a corrosion weight loss rate of less than 0.5 g / m in a 3.5% NaCl salt spray environment. 2 .h, the polishing grade reaches PLASTICS A2 standard, and the production of extra-thick modules for corrosion-resistant molds with a thickness of 200 to 600 mm is achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the core structure of the 600mm thick composite extra-thick module of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] The chemical composition of the steel grades of the embodiments of the present invention is shown in Table 1, the processing parameters of the continuous casting billet of the embodiments are shown in Table 2, the processing parameters of the single-wire gas-electric vertical welding billet of the embodiments are shown in Table 3, the forging process of the embodiments is shown in Table 4, the heat treatment process of the embodiments is shown in Table 5, and the actual effects of the embodiments are shown in Tables 6 and 7.

[0032] Table 1 Chemical composition of steel smelting in each example (%)

[0033]

[0034]

[0035] Table 2 Processing parameters of continuous casting billets in various embodiments

[0036]

[0037] Table 3 Process parameters of welding assembly in various embodiments

[0038]

[0039] Table 4 Forging process parameters of each embodiment

[0040]

[0041] Table 5 Heat treatment process parameters of each embodiment

[0042]

[0043]

[0044] Table 6 Actual effects of various embodiments

[0045]

[0046] Table 7 Actual effects of various embodiments

[0047]

[0048] See Figure 1 It is the metallographic structure diagram of Example 2, from Figure 1 It can be seen that the core structure of the extra-thick module of the present invention is tempered troostite, and the composite interface achieves good metallurgical bonding.

Claims

1. A method for producing extra-thick modular steel for corrosion-resistant molds, characterized in that: The method comprises the following steps: 1) Preheating of composite billet before welding: Align the surfaces of the processed continuous casting billets to be composited, stack them up and down, and use electric heating asbestos pads to cover the billets around them and preheat them. The preheating temperature is 200-300℃ and the preheating time is 3-4h. 2) Welding: The welding adopts the single-wire gas-electric vertical welding method, and the welding is carried out along the four sides of the billet. The wire speed is 10-15m / min, the CO2 gas flow rate is 20-30L / min, the cooling water flow rate is ≥2L / min, the welding current is 280-380A, the arc voltage is 34-40V, the welding speed is 15-25cm / min, and the weld seam exhaust hole is reserved. Then a vacuum pump is used to extract the vacuum from the weld seam exhaust hole to a vacuum degree of ≤1Pa, and then spot welding is used to complete the sealing; 3) Post-weld heating: After welding is completed, the weld area is again heated with an electric heating asbestos pad at a temperature of 150-200°C for 4-5 hours. The composite blank is then hoisted to the heating furnace for heating. The surface temperature of the composite blank is not less than 100°C when loaded into the furnace. 4) Heating forging: Two-fire heating forging is adopted, the target heating temperature is 1200℃~1240℃, the first fire heating time is 1.5~2h / 100mm thickness, and the second fire heating to the target heating temperature is kept warm for 2.5~4h; After the billet is taken out of the furnace, water mist is used to cool its upper surface, the water temperature of the water mist is ≤35℃, the volume ratio of water to air in the water mist is 1:180~1:220, and the cooling temperature is 800~850℃; a 3000-ton hydraulic press is used to forge the composite billet, and the upper and lower hammers are of asymmetric size; the upper hammer adopts a flat hammer head with a width of W=0.4~0.5H and a length of L=1.5~1.8W′, and the width of the lower forging platform is ≥2.0W′, where H and W′ are the height and width of the composite billet respectively; the initial forging temperature is ≥1150℃ at 1 / 2 of the billet thickness, and the final forging temperature is ≥800℃ at 1 / 2 of the billet thickness. The product is forged in two fires, with a total forging ratio of 1.5~2, and a single-pass forging feed of 0.8~1.0W. After forging, it is air-cooled to room temperature; 5) Heat treatment: The heat treatment adopts water mist-air alternating time-controlled quenching + tempering process. The water mist-air alternating time-controlled quenching process is: heating temperature 1000-1050℃, net holding time 1-1.4min / mm thickness, then air cooling for 15-25min → water mist cooling for 20-40min → air cooling for 50-70min, water mist cooling for 1.5-3h → air cooling to room temperature, tempering temperature 610℃-640℃, holding time 5-7min / mm thickness; The chemical composition of the steel is calculated by weight percentage: C 0.20%~0.45%, Si≤1.0%, Mn≤1.0%, Cr 10.5%~18.0%, Ni≤1.20%, Mo≤1.2%, V≤0.50%, P≤0.040%, S≤0.050%, and the rest is Fe and unavoidable impurities; The finished thickness of the extra-thick modular steel for corrosion-resistant molds is 300 to 600 mm.

2. The method for producing extra-thick modular steel for corrosion-resistant molds according to claim 1, characterized in that: The surface of the continuous casting billet to be composited after slow cooling and destacking is milled and ground to remove the oxide layer and rust layer; after milling and grinding, the gap between the continuous casting billets is ≤2mm, and the surface roughness Ra is ≤50µm.

3. The method for producing extra-thick module steel for corrosion-resistant molds according to claim 2, characterized in that: Before preheating the composite billet before welding, the four sides of the composite surface to be processed are chamfered, and the chamfering size is (15 ~ 20mm) × (40 ~ 50) °.

4. The method for producing extra-thick modular steel for corrosion-resistant molds according to claim 1, characterized in that: The continuous casting billets which are more than 3m away from the head and tail of the continuous casting billets are selected as the billets to be composited. After the continuous casting billets come off the line, they are stacked and slowly cooled. The stacking temperature is ≥650℃ and the stacking time is ≥48h.

5. The method for producing extra-thick modular steel for corrosion-resistant molds according to claim 1, characterized in that: In the water mist in the above step 5), the water temperature is ≤35°C, and the volume ratio of water to air is 1:450 to 1:

470.

6. The method for producing extra-thick modular steel for corrosion-resistant molds according to claim 1, characterized in that: The corrosion weight loss rate of module steel in 3.5% NaCl salt spray environment is less than 0.5g / m 2 .h.