A kind of solidifying agent for shield mud and preparation method thereof

Through the combination of fly ash, coal burning waste residue and alkali liquid, the problem of long curing time and low strength of shield mud curing agent is solved, and the rapid solidification and strength improvement of shield mud is achieved, meeting the needs of the construction site and reducing costs. and environmental load.

CN116177909BActive Publication Date: 2024-10-18TENGDA CONSTR GROUP CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310209287.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-10-18
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Existing shield mud curing agents have problems such as long curing time and low strength.

Method used

A specific combination of fly ash, coal combustion waste residue and alkali liquid is used as the solidifying agent, prepared through primary and secondary reactions, to achieve rapid solidification of shield mud and significantly improve the strength of the solidified soil.

Benefits of technology

While meeting the operational time requirements on the construction site, it significantly improves the strength of the mud-solidified soil, reduces costs, and improves environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004112018280000091
    Figure BDA0004112018280000091
  • Figure BDA0004112018280000101
    Figure BDA0004112018280000101
  • Figure BDA0004112018280000111
    Figure BDA0004112018280000111
Patent Text Reader

Abstract

The present invention relates to a curing agent for shield mud and a preparation method thereof, wherein the curing agent comprises fly ash, coal waste residue and alkali solution in a mass ratio of (18-38):1:(5-10). The preparation process is that after the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once, and then the alkali residue mixture is obtained and then the fly ash is reacted twice to obtain the curing agent. The curing agent provided by the present invention realizes the preparation of the curing agent used for curing the shield mud by adopting a specific combination of coal waste residue, fly ash and alkali, can react quickly with the waste mud water when the operation time requirement of the construction site is met, and significantly improves the strength of the mud solidified soil, greatly reduces the cost, and improves the environmental benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid waste treatment, and in particular to a curing agent for shield mud and a preparation method thereof. Background Art

[0002] At present, ordinary Portland cement is the most widely used solidifying cementitious material in modern society. However, its preparation process, often referred to as "two grindings and one burning", has been criticized for its high greenhouse gas emissions and energy consumption. If not improved, it will lead to more serious environmental problems in the foreseeable future. Therefore, it is crucial to find a greener alternative to ordinary Portland cement. Alkali-activated materials, including geopolymers, have a reputation for their green manufacturing and excellent mechanical properties. These materials can be used as cement or in concrete and mortar, and alkali-activated materials have good results in terms of mechanical strength and durability.

[0003] In the process of urban construction, a large amount of waste mud is generated. However, waste shield mud generally has a high water content and is difficult to stack. On-site drying occupies land resources and is difficult to transport, which causes great pollution to the environment. In addition, the special floc structure and high hydrophilicity of waste shield mud particles make it difficult to remove the water they contain. If a dehydration process is used, it will not only be inefficient but also costly. The volume of waste shield mud is large and subsequent treatment is difficult. However, if it is not properly handled, it will endanger the surrounding ecological environment.

[0004] In the prior art, it is proposed to treat shield mud by solidification, such as CN110194577A discloses a shield mud solidifier, which includes the following components by weight: 10-20 parts of calcium oxide, 3-8 parts of white carbon black, 0.3-1.2 parts of cellulose and 7-15 parts of sepiolite loaded with iron salt. The shield mud solidifier provided by the scheme is composed of calcium oxide, white carbon black, cellulose and sepiolite loaded with iron salt, and the mass ratio of each component is optimized and designed so that each component works synergistically, so that the shield mud can be dehydrated and solidified quickly and efficiently, and the solidification effect of the shield mud is significantly improved; by using sepiolite as a carrier of iron salt, the shield mud solidifier has the effects of flocculation and solidification at the same time, which significantly enhances the solidification treatment effect of the shield mud.

[0005] CN109456010A discloses a shield construction waste mud curing agent prepared by using oil refining solid waste and a method of using the same. The characteristics are as follows: the shield construction waste mud curing agent is mixed with component A and component B, wherein component A is the main material, including petroleum coke desulfurization ash and cement, wherein the petroleum coke desulfurization ash accounts for 55%-80% of the total weight, and the cement accounts for 5%-26% of the total weight. Component B is the auxiliary material, including water glass, polyacrylamide and polyferric sulfate, wherein the water glass accounts for 0-16% of the total weight, and the sum of polyacrylamide and polyferric sulfate accounts for 1%-3% of the total weight. When used, the shield construction waste mud curing agent in the bag is sprinkled into the shield construction waste mud to be cured and stirred, so that the shield construction waste mud is converted into a solidified body, and a dry and formed slurry block is obtained after standing for a period of time. The curing agent solidifies the subway shield construction waste mud, which can treat waste with waste, and achieve the purpose of dual resource utilization of waste sludge and oil refining solid waste.

[0006] However, existing curing agents still have the problems of long curing time and low strength. Summary of the invention

[0007] In view of the problems existing in the prior art, the object of the present invention is to provide a curing agent for shield mud and a preparation method thereof, so as to solve the problems that the curing agent used still has a long curing time and low strength.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a curing agent for shield mud, wherein the curing agent comprises fly ash, coal combustion waste residue and alkali solution in a mass ratio of (18-38):1:(5-10).

[0010] The curing agent provided by the present invention realizes the preparation of the curing agent used for shield mud curing by adopting a specific combination of coal combustion waste residue, fly ash and alkali. It can react quickly with the waste mud water while meeting the on-site operability time requirements, and significantly improves the strength of mud-cured soil, greatly reducing costs and improving environmental benefits.

[0011] In the present invention, the mass ratio of the fly ash, coal combustion waste residue and alkali solution is (18-38):1:(5-10), for example, it can be 18:1:5, 19:1:5, 20:1:5, 21:1:5, 22:1:5, 23:1:5, 24:1:5, 25:1:5, 26:1:5, 27:1:5, 28:1:5, 29:1:5, 30:1:5, 32:1:5, 34:1:5, 36:1:5, 38:1:5, 18:1:6, 18:1:7, 18:1:8, 18:1:9 or 18:1:10, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0012] In the present invention, the water content of the shield mud is 25-35%, for example, it can be 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34% or 35%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0013] In the present invention, the modulus of sodium silicate in the obtained curing agent can be controlled to be 1.0, 1.2 or 1.5.

[0014] As a preferred technical solution of the present invention, the alkali solution includes sodium hydroxide solution and / or potassium hydroxide solution.

[0015] Preferably, the molar concentration of the alkali solution is 8-12 mol / L, for example, it can be 8 mol / L, 8.1 mol / L, 8.2 mol / L, 8.3 mol / L, 8.4 mol / L, 8.5 mol / L, 8.6 mol / L, 8.7 mol / L, 8.8 mol / L, 8.9 mol / L, 9 mol / L, 9.1 mol / L, 9.2 mol / L, 9.3 mol / L, 9.4 mol / L, 9.5 mol / L, 9.6 mol / L, 9.7 mol / L, 9.8 mol / L, 9.9 mol / L, 10 mol / L, 10.1 mol / L, 1 / L, 10.2mol / L, 10.3mol / L, 10.4mol / L, 10.5mol / L, 10.6mol / L, 10.7mol / L, 10.8mol / L, 10.9mol / L, 11mol / L, 11.1mol / L, 11.2mol / L, 11.3mol / L, 11.4mol / L, 11.5mol / L, 11.6mol / L, 11.7mol / L, 11.8mol / L, 11.9mol / L or 12mol / L, but are not limited to the listed values, and other unlisted values ​​within the range are equally applicable.

[0016] As a preferred technical solution of the present invention, the fly ash comprises SiO2 55-62%, Al2O3 10-12%, and CaO 6-7% by mass percentage;

[0017] In the present invention, the mass percentage of SiO2 in the fly ash is 55-62%, for example, it can be 55%, 55.5%, 56%, 56.5%, 57%, 57.5%, 58%, 58.5%, 59%, 59.5%, 60%, 60.5%, 61%, 61.2% or 62%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0018] In the present invention, the mass percentage of Al2O3 in the fly ash is 10-12%, for example, it can be 10%, 10.1%, 10.2%, 10.3%, 10.4%, 10.5%, 10.6%, 10.7%, 10.8%, 10.9%, 11%, 11.1%, 11.2%, 11.3%, 11.4%, 11.5%, 11.6%, 11.7%, 11.8%, 11.9% or 12%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0019] In the present invention, the mass percentage of CaO in the fly ash is 6-7%, for example, it can be 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9% or 7%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0020] Preferably, the mass percentage of SiO2 in the coal-fired waste slag is 60-63%, for example, it can be 60%, 60.1%, 60.2%, 60.3%, 60.4%, 60.5%, 60.6%, 60.7%, 60.8%, 60.9%, 61%, 61.1%, 61.2%, 61.3%, 61.4%, 61.5%, 61.6%, 61.7%, 61.8%, 61.9%, 62%, 62.1%, 62.2%, 62.3%, 62.4%, 62.5%, 62.6%, 62.7%, 62.8%, 62.9% or 63%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0021] In the present invention, fly ash and coal waste residue are both materials produced after biomass combustion, and the difference lies in the obvious difference in particle size and content of specific substances. In addition to unburned coal particles, the material also contains a large amount of silicon, iron, aluminum, calcium, magnesium, sodium, potassium, sulfur oxides and various trace elements. The main phase is glass, accounting for 50%-80%; the crystal minerals contained are mullite, α-quartz, calcite, calcium feldspar, calcium silicate, hematite and magnetite, etc., and a small amount of unburned carbon.

[0022] In a second aspect, the present invention provides a method for preparing the curing agent according to the first aspect, the preparation method comprising:

[0023] After the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once to obtain the alkali residue mixture, which is then reacted with fly ash for a secondary reaction to obtain the curing agent.

[0024] As a preferred technical solution of the present invention, the particle size of the coal-fired waste slag is 75-5000 μm.

[0025] As a preferred technical solution of the present invention, the particle size of the fly ash is 5-90 μm.

[0026] In the present invention, the particle size of coal waste residue and fly ash refers to a particle cluster in any interval within a range, that is, when specifically selected, the interval that can be selected for fly ash is 5-90μm, 5-10μm, 7-15μm, 12-20μm, 18-30μm, 25-37μm, 32-45μm, 42-58μm, 53-64μm, 60-76μm, 72-83μm or 40-90μm, etc. For example, the interval that can be selected for coal waste residue is 75-100μm, 80-500μm, 300-800μm, 1000-2000μm, 2000-5000μm, 1800-3000μm, 90-1000μm or 220-400μm, etc., but it is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0027] As a preferred technical solution of the present invention, the temperature of the primary reaction is 120-140°C, for example, it can be 120°C, 122°C, 124°C, 126°C, 128°C, 130°C, 132°C, 134°C, 136°C, 138°C or 140°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0028] Preferably, the time of the primary reaction is 4-5 h, for example, 4 h, 4.2 h, 4.4 h, 4.6 h, 4.8 h or 5 h, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0029] As a preferred technical solution of the present invention, the alkali in the alkali slag mixture in the secondary reaction is 6-7% of the mass of the fly ash in terms of sodium oxide, for example, it can be 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9% or 7%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are equally applicable.

[0030] In the present invention, the time and temperature parameters of the secondary reaction can be selected according to actual conditions. The time of the secondary reaction can be 2-3 hours, and the temperature of the secondary reaction can be 50-75°C.

[0031] As a preferred technical solution of the present invention, the preparation method comprises: reacting coal waste residue and alkali solution once after mixing according to the formula to obtain an alkali residue mixture, and then reacting the mixture with fly ash for a second time to obtain the curing agent.

[0032] The particle size of the coal-fired waste residue is 75-5000 μm; the particle size of the fly ash is 5-90 μm;

[0033] ; The temperature of the primary reaction is 120-140°C; The time of the primary reaction is 4-5h;

[0034] In the secondary reaction, the sodium oxide in the alkali slag mixture accounts for 6-7% of the mass of the fly ash.

[0035] In the present invention, the amount of curing agent added during use is based on the dry matter mass in the shield mud, and can be 12-18% of the dry matter mass in the shield mud, for example, it can be 12%, 12.2%, 12.4%, 12.6%, 12.8%, 13%, 13.2%, 13.4%, 13.6%, 13.8%, 14%, 14.2%, 14.4%, 14.6%, 14.8%, 15%, 15.2%, 15.4%, 15.6%, 15.8%, 16%, 16.2%, 16.4%, 16.4%, 16.6%, 16.8%, 17%, 17.2%, 17.4%, 17.6%, 17.8% or 18%, etc., but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0036] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0037] (1) The present invention provides a new type of cementitious material having high durability and low environmental load, which is prepared by combining fly ash and ground granulated blast furnace slag powder (hereinafter referred to as slag). The fluidity of mud lies in the fact that there is too much free water between soil particles and the friction between soil particles is too small, so that soil particles can move freely. By adding a curing agent to bond soil particles, the soil particles that were originally free to move are bonded into a whole, thereby solidifying the mud. The larger the bonding area between soil particles, the stronger the integrity between soil particles and the higher the strength.

[0038] (2) After curing, the compressive strength of the obtained solidified product is 0.3-3MPa, which improves the construction efficiency, simplifies the construction process, and has good economic benefits. The preparation process does not involve calcination and does not produce harmful gases. Under the action of the activator, the industrial waste residue converts the free water in the system into bound water and fixes it. The soil particles are connected as a whole through the CASH gel, which has good economic and environmental benefits. DETAILED DESCRIPTION

[0039] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0040] Example 1

[0041] The present embodiment provides a curing agent for shield mud, the curing agent comprises fly ash, coal-fired waste residue and alkali solution, the mass ratio of which is 24.8:1:8.3, the alkali solution is a sodium hydroxide solution, the molar concentration of the alkali solution is 10 mol / L, the fly ash comprises SiO2 59%, Al2O3 11%, and CaO 6.5% by mass percentage, and the SiO2 in the coal-fired waste residue is 62% by mass percentage;

[0042] The specific preparation process is as follows:

[0043] After the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once to obtain the alkali residue mixture, which is then reacted with fly ash for a secondary reaction to obtain the curing agent.

[0044] The particle size of the coal-fired waste residue is 75-200 μm; the particle size of the fly ash is 5-50 μm;

[0045] The temperature of the primary reaction is 130°C; the time of the primary reaction is 4.5h;

[0046] In the secondary reaction, the sodium oxide in the alkali slag mixture is 6.5% of the mass of the fly ash; the temperature of the secondary reaction is 50° C.; and the time of the secondary reaction is 2 hours.

[0047] Example 2

[0048] The present embodiment provides a curing agent for shield mud, the curing agent comprises fly ash, coal-fired waste residue and alkali solution, the mass ratio of which is 21.1:1:8.4, the alkali solution is a sodium hydroxide solution, the molar concentration of the alkali solution is 8 mol / L, the fly ash comprises SiO2 62%, Al2O3 12%, and CaO 6% by mass percentage, and the SiO2 in the coal-fired waste residue is 60% by mass percentage;

[0049] The specific preparation process is as follows:

[0050] After the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once to obtain the alkali residue mixture, which is then reacted with fly ash for a secondary reaction to obtain the curing agent.

[0051] The particle size of the coal-fired waste residue is 2000-5000 μm; the particle size of the fly ash is 40-90 μm;

[0052] The temperature of the primary reaction is 140°C; the time of the primary reaction is 5h;

[0053] The sodium oxide in the alkali slag mixture in the secondary reaction is 6% of the mass of the fly ash; the temperature of the secondary reaction is 75° C.; and the time of the secondary reaction is 3 hours.

[0054] Example 3

[0055] The present embodiment provides a curing agent for shield mud, the curing agent comprises fly ash, coal-fired waste residue and alkali solution, the mass ratio of which is 28.1:1:8.3, the alkali solution is a potassium hydroxide solution, the molar concentration of the alkali solution is 12 mol / L, the fly ash comprises SiO2 55%, Al2O3 10%, and CaO 7% by mass percentage, and the SiO2 in the coal-fired waste residue is 63% by mass percentage;

[0056] The specific preparation process is as follows:

[0057] After the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once to obtain the alkali residue mixture, which is then reacted with fly ash for a secondary reaction to obtain the curing agent.

[0058] The particle size of the coal-fired waste residue is 100-1500 μm; the particle size of the fly ash is 30-65 μm;

[0059] The temperature of the primary reaction is 120°C; the time of the primary reaction is 4h;

[0060] In the secondary reaction, the sodium oxide in the alkali slag mixture is 7% of the mass of the fly ash; the temperature of the secondary reaction is 50° C.; and the time of the secondary reaction is 2 hours.

[0061] Example 4

[0062] The present embodiment provides a curing agent for shield mud, the curing agent comprises fly ash, coal-fired waste residue and alkali solution, the mass ratio of which is 23:1:8.3, the alkali solution comprises sodium hydroxide solution and / or potassium hydroxide solution, the molar concentration of the alkali solution is 9 mol / L, the fly ash comprises SiO2 58%, Al2O3 11%, and CaO 6.3% by mass percentage, and the SiO2 in the coal-fired waste residue is 61.5% by mass percentage;

[0063] The specific preparation process is as follows:

[0064] After the ingredients are prepared according to the formula, the coal waste residue and the alkali solution are reacted once to obtain the alkali residue mixture, which is then reacted with fly ash for a secondary reaction to obtain the curing agent.

[0065] The particle size of the coal-fired waste residue is 150-350 μm; the particle size of the fly ash is 6-20 μm;

[0066] The temperature of the primary reaction is 128°C; the time of the primary reaction is 4.7h;

[0067] The sodium oxide in the alkali slag mixture in the secondary reaction is 6.8% of the mass of the fly ash; the temperature of the secondary reaction is 75° C.; and the time of the secondary reaction is 3 hours.

[0068] Example 5

[0069] The difference from Example 1 is only that the alkali solution is replaced by an equal amount of sodium carbonate solution of equal concentration.

[0070] Example 6

[0071] The only difference from Example 1 is that the fly ash is replaced by water glass having the same silicon dioxide content as that in the fly ash.

[0072] Example 7

[0073] The only difference from Example 1 is that the coal-fired waste residue is replaced by water glass having the same silicon dioxide content as that in the coal-fired waste residue.

[0074] Example 8

[0075] The only difference from Example 1 is that the coal-fired waste residue is replaced by an equal amount of fly ash.

[0076] Example 9

[0077] The only difference from Example 1 is that the fly ash is replaced by an equal amount of coal-fired waste slag.

[0078] Application Example 1

[0079] The curing agent obtained in the above examples 1-9 is reacted with shield mud with a water content of 30%, and the addition amount of the curing agent is 5%, 10%, 15%, 18% and 20% of the dry matter mass in the shield mud, respectively, and then briquettes are made under a pressure of 20MPa. The obtained solidified product is tested for compressive strength mechanical properties according to ASTM C109 / C109M-2016a, and the specific data are shown in Table 1. The fly ash and coal waste residue in the above examples are obtained by sorting secondary Class C fly ash.

[0080] Table 1

[0081]

[0082]

[0083]

[0084]

[0085] It can be seen from the results of the above embodiments and comparative examples that the curing agent provided by the present invention realizes the preparation of the curing agent used for shield mud curing by adopting a specific combination of coal combustion waste slag, fly ash and alkali. It can react quickly with the waste mud water while meeting the on-site operational time requirements, and significantly improve the strength of the mud-cured soil, greatly reducing costs and improving environmental benefits.

[0086] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0087] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0088] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0089] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A curing agent for shield mud, characterized in that: The curing agent is composed of fly ash, coal combustion waste residue and alkali solution in a mass ratio of (18-38):1:(5-10); The alkali solution includes sodium hydroxide solution and / or potassium hydroxide solution; The preparation method of the curing agent is as follows: After the ingredients are prepared according to the formula, the coal-fired waste residue and the alkali solution are reacted once to obtain an alkali-slag mixture, and then the mixture is reacted with fly ash for a secondary reaction to obtain the curing agent; The temperature of the primary reaction is 120-140°C; the time of the primary reaction is 4-5h; The temperature of the secondary reaction is 50-75° C.; the time of the secondary reaction is 2-3 hours.

2. The curing agent according to claim 1, characterized in that The molar concentration of the alkali solution is 8-12 mol / L.

3. The curing agent according to claim 1, characterized in that The fly ash comprises SiO2 55-62%, Al2O3 10-12%, and CaO 6-7% in terms of mass percentage.

4. The curing agent according to claim 1, characterized in that The mass percentage of SiO2 in the coal-fired waste slag is 60-63%.

5. The curing agent according to claim 1, characterized in that The particle size of the coal-fired waste slag is 75-5000 μm.

6. The curing agent according to claim 1, characterized in that The particle size of the fly ash is 5-90 μm.

7. The curing agent according to claim 1, characterized in that In the secondary reaction, the alkali in the alkali slag mixture is 6-7% of the mass of the fly ash in terms of sodium oxide.

Citation Information

Patent Citations

  • Shield construction waste slurry curing agent prepared from oil refining solid wastes and use method

    CN109456010A

  • Shield mud solidifying agent, preparation method and application method thereof

    CN110194577A

  • Novel composite polymer shield muck curing agent

    CN115650690A