A high-strength, high-elongation aluminum foil and its applications
By controlling the grain size and rolling texture of the aluminum foil, and preparing by casting and rolling method, the problems of insufficient strength and elongation of the existing aluminum alloy foil are solved, and high-strength and high elongation aluminum foil are achieved, suitable for lithium ion Battery current collector.
Patent Information
- Application Number
- CN202211538085.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-02
AI Technical Summary
The existing aluminum alloy foil for positive electrode current collector cannot achieve high strength and high elongation at the same time, and cannot meet the stability of lithium-ion batteries and improve the energy density of the battery during compaction under high pressure conditions.
Through EBSD detection, the grain size of aluminum foil is ≤6μm and the rolled texture account for 55%~76%. It is prepared by casting and rolling method, and combined with the difference between cast-rolling coil and intermediate annealing thickness, the grain size and texture are controlled. Distribution to improve the strength and elongation of aluminum foil.
The high strength (256~277 MPa) and high elongation (4.3%~4.9%) of aluminum foil are achieved, meeting the performance requirements of lithium-ion battery current collectors.
Smart Images

Figure CN116179897B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum-based alloys, and more specifically, to a high-strength and high-elongation aluminum foil and application thereof. Background Art
[0002] At present, the positive electrode current collector in lithium-ion batteries is mainly prepared by coating the positive electrode material with aluminum foil as the substrate. Moreover, with the continuous advancement of lithium-ion battery technology, the market demand for the energy density and safety performance of lithium-ion batteries is getting higher and higher, and the positive electrode material plays a key role in the energy density and safety of lithium-ion batteries.
[0003] As a lithium-ion battery manufacturer, a higher compaction density of positive electrode materials is usually used to improve the energy density of the battery, but this also increases the requirements for aluminum foil accordingly. There is an urgent need for aluminum foil to have higher strength and elongation so that the aluminum foil can better adapt to the compaction process of positive electrode materials under high pressure conditions without breaking the foil or reducing the number of foil breaks.
[0004] For example, the prior art provides a high-strength aluminum alloy foil for positive electrode current collector and a method for manufacturing the same, wherein an appropriate amount of Fe element is added to the aluminum foil to achieve both conductivity and strength of the aluminum alloy; a small amount of Mn element is further used for solid solution strengthening to improve the strength of the aluminum alloy; an appropriate amount of La element is added to refine the alloy grains and promote Al in the aluminum alloy. 3 The fine spherical precipitation of the Fe second phase inhibits the irregular large Fe-containing precipitate phase, and at the same time generates a new AlFeLa phase to further strengthen the alloy. Although the strength of the aluminum alloy foil is improved, the elongation of the aluminum alloy foil is low (1.02%~1.38%).
[0005] In addition, in order to ensure the excellent conductivity of aluminum foil, the prior art usually adopts pure aluminum 1XXX series aluminum foil to ensure excellent conductivity, and basically adopts battery aluminum foil with grades of 1050 / 1060 / 1070. However, the strength of these grades of battery aluminum foil is usually relatively low, and most of them have a tensile strength of ≤220MPa, which cannot meet the energy density development trend of future lithium batteries. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects and shortcomings of the existing aluminum alloy foil for positive electrode current collector that cannot achieve high strength and high elongation at the same time, and to provide a high-strength and high-elongation aluminum foil.
[0007] Another object of the present invention is to provide application of the above-mentioned high-strength and high-elongation aluminum foil in battery current collectors.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A high-strength and high-elongation aluminum foil. The grain size of the aluminum foil with a thickness of 0.010-0.020 mm is determined by EBSD detection means to be ≤6 μm, and the rolling texture of the aluminum foil accounts for 55%-76%.
[0010] The high-strength and high-elongation aluminum foil of the present invention achieves higher strength and improves its elongation by matching grains of a specific size with rolling textures of an appropriate proportion. If the grain size is too large, the strength of the aluminum foil will decrease; if the rolling texture of the aluminum foil accounts for too large a proportion, although the strength can be improved, the elongation of the aluminum foil will be significantly reduced, and the production and processing rolling performance will be poor; if the rolling texture of the aluminum foil accounts for too small a proportion, the elongation and strength of the aluminum foil will both decrease, making it difficult to meet application requirements.
[0011] The rolling texture percentage of the aluminum foil of the present invention is measured by an EBSD instrument, and the sum of the annealing texture and the rolling texture is 100%.
[0012] Preferably, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.5-5.6 μm.
[0013] Preferably, the rolling texture of the aluminum foil accounts for 60% to 75%.
[0014] In a specific embodiment, the aluminum foil of the present invention comprises the following components by mass percentage:
[0015] Si: 0.03%~0.09%, Fe: 0.52%~0.7%, Cu: 0.09%~0.22%, Zn≤0.03%, Ti: 0.015%~0.025%, other single impurity elements ≤0.05%, the balance is aluminum.
[0016] It should be noted that by controlling the composition of the aluminum foil so that the ratio of Fe / Si elements is appropriate, the second phase compound generated by the casting and rolling process is finer and more uniform, thereby better regulating the grain size of the aluminum foil.
[0017] In a specific embodiment, the high-strength and high-elongation aluminum foil is prepared by a casting and rolling method, which specifically includes the following steps:
[0018] First, the aluminum foil raw material is successively smelted and cast-rolled to form a cast-rolled coil; then it is successively cold-rolled, intermediate annealed and foil-rolled to obtain a high-strength and high-elongation aluminum foil;
[0019] The thickness of the intermediate annealing is 40% to 59% of the thickness of the cast-rolled coil, and the thickness of the high-strength and high-elongation aluminum foil is 0.4% to 5% of the thickness of the intermediate annealing.
[0020] By controlling the difference between the thickness of the cast-rolled coil and the intermediate annealing thickness, the Si and Fe elements can obtain the best precipitation conditions, improve the uniformity of the deformation storage energy distribution in the thickness direction of the aluminum foil and the uniformity of the recrystallized grain growth, thereby improving the grain size of the annealing structure, and thus making the prepared aluminum foil have high elongation while meeting the requirements of high strength; at the same time, by controlling the difference between the intermediate annealing thickness and the thickness of the high-strength and high-elongation aluminum foil, a large amount of rolling texture can be retained in the aluminum foil, so that the grains are broken into more uniform and fine grains after work hardening, and combined with the solid solution amount of the Cu element, the aluminum foil can be given high strength, so that the final aluminum foil has high strength and high elongation.
[0021] Specifically, the intermediate annealing treatment is performed only once.
[0022] Preferably, the thickness of the intermediate annealing is 45% to 55% of the thickness of the cast-rolled coil.
[0023] Preferably, the thickness of the high-strength and high-elongation aluminum foil is 0.4% to 2% of the intermediate annealing thickness.
[0024] Specifically, the grain structures of the surface, cross section and longitudinal section after intermediate annealing are uniform, wherein the average grain size of the surface is 100-300 μm; the average grain size of the cross section is ≤100 μm; and the average grain size of the longitudinal section is ≤100 μm.
[0025] The grain size distribution of the aluminum coil after intermediate annealing in its thickness direction is different. The surface annealing grain size is the largest, and the influence of grains of different sizes on the material strength is different. When the average grain size of surface annealing is 100~300μm, the average grain size of cross-section annealing is ≤100μm, and the average grain size of longitudinal section annealing is ≤100μm, the strength and elongation of the aluminum foil can be better improved.
[0026] Preferably, the grain structure of the surface, cross section and longitudinal section after intermediate annealing is uniform, wherein the average grain size of the surface is 100-200 μm; the average grain size of the cross section is 70-95 μm; and the average grain size of the longitudinal section is 70-95 μm.
[0027] Specifically, the intermediate annealing temperature is 300-450° C., the holding time is 4-8 hours, and the heating rate from room temperature to the required annealing temperature is ≥40° C. / h.
[0028] When the intermediate annealing temperature is 300~450℃ and the holding time is 4~8h, recrystallized grains can be effectively formed; at the same time, the grain growth during the annealing process can be prevented to form secondary recrystallized grains, thereby greatly improving the strength and elongation of the final aluminum foil. In addition, when the heating rate is ≥40℃ / h, the annealing grain structure can be made more uniform, and the grain growth can be prevented to the greatest extent, thereby improving the strength and elongation of the aluminum foil.
[0029] Preferably, the intermediate annealing temperature is 320-400° C., the holding time is 4-8 hours, and the heating rate from room temperature to the required annealing temperature is ≥50° C. / h.
[0030] The application of the above-mentioned high-strength and high-elongation aluminum foil in lithium-ion batteries is also within the protection scope of the present invention.
[0031] Compared with the prior art, the present invention has the following beneficial technical effects:
[0032] The present invention provides a high-strength and high-elongation aluminum foil, wherein the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is ≤6 μm, the rolling texture of the aluminum foil accounts for 55%-76%, and the aluminum foil has high strength and high elongation.
[0033] The strength reaches 256~277 MPa and the elongation reaches 4.3%~4.9%.
[0034] The above-mentioned aluminum foil is prepared by a casting and rolling method. By controlling the thickness difference between the cast-rolled coil formed by casting and rolling and the intermediate annealing thickness, as well as the thickness difference between the intermediate annealing thickness and the high-strength and high-elongation aluminum foil, the deformation storage energy of the high-strength and high-elongation aluminum foil in the thickness direction is evenly distributed, and the grains formed by recrystallization grow evenly, thereby improving the annealing structure and controlling the grain structure within a reasonable range, thereby achieving the goal of improving the strength of the aluminum foil while improving its elongation. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the surface grain structure diagram after intermediate annealing treatment in Example 1.
[0036] Figure 2 This is the grain structure diagram within the surface range of the cross section after intermediate annealing treatment in Example 1.
[0037] Figure 3 This is the grain structure diagram within the center layer of the cross section after intermediate annealing treatment in Example 1.
[0038] Figure 4 This is the grain structure diagram within the surface range of the longitudinal section after intermediate annealing treatment in Example 1.
[0039] Figure 5This is the grain structure diagram within the central layer of the longitudinal section after intermediate annealing treatment in Example 1.
[0040] Figure 6 The grain sizes at different positions of the high-strength and high-elongation aluminum foil in Example 5.
[0041] Figure 7 The grain sizes at different positions of the high-strength and high-elongation aluminum foil in Example 6.
[0042] Figure 8 and Fig. 9 This is the texture distribution diagram of different positions of the high-strength and high-elongation aluminum foil in Example 1. DETAILED DESCRIPTION
[0043] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0044] Example 1
[0045] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.6 μm, and the rolling texture of the aluminum foil accounts for 65%.
[0046] Aluminum foil includes the following components by mass percentage:
[0047] Si: 0.06%, Fe: 0.56%, Cu: 0.14%, Zn: 0.02%, Ti: 0.016%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0048] The above-mentioned high-strength and high-elongation aluminum foil can be prepared by the following preparation method:
[0049] First, the aluminum foil raw material is successively smelted and cast-rolled to form a cast-rolled coil; then it is successively cold-rolled, intermediate annealed and foil-rolled to obtain a high-strength and high-elongation aluminum foil;
[0050] The intermediate annealing temperature is 400°C and the time is 4h;
[0051] The intermediate annealing thickness is 55% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 45%), and the thickness of the high-strength and high-elongation aluminum foil is 1.5% of the intermediate annealing thickness (equivalent to a thickness difference of 98.5%).
[0052] The intermediate annealing temperature is increased from room temperature to the desired annealing temperature at a heating rate of 40° C. / h.
[0053] Example 2
[0054] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 5.5 μm, and the rolling texture of the aluminum foil accounts for 69%.
[0055] Aluminum foil includes the following components by mass percentage:
[0056] Si: 0.09%, Fe: 0.52%, Cu: 0.20%, Zn: 0.01%, Ti: 0.015%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0057] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 49% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 51%), and the thickness of the high-strength and high-elongation aluminum foil is 0.7% of the intermediate annealing thickness (equivalent to a thickness difference of 99.3%).
[0058] Example 3
[0059] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 5.6 μm, and the rolling texture of the aluminum foil accounts for 58%.
[0060] Aluminum foil includes the following components by mass percentage:
[0061] Si: 0.03%, Fe: 0.6%, Cu: 0.09%, Zn: 0.03%, Ti: 0.018%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0062] The method for preparing the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 59% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 41%), and the thickness of the high-strength and high-elongation aluminum foil is 1.1% of the intermediate annealing thickness (equivalent to a thickness difference of 98.9%).
[0063] Example 4
[0064] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.5 μm, and the rolling texture of the aluminum foil accounts for 70%.
[0065] Aluminum foil includes the following components by mass percentage:
[0066] Si: 0.05%, Fe: 0.65%, Cu: 0.12%, Zn: 0.025%, Ti: 0.024%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0067] The method for preparing the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 40% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 60%), and the thickness of the high-strength and high-elongation aluminum foil is 0.9% of the intermediate annealing thickness (equivalent to a thickness difference of 99.1%).
[0068] Example 5
[0069] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.6 μm, and the rolling texture of the aluminum foil accounts for 69%.
[0070] Aluminum foil includes the following components by mass percentage:
[0071] Si: 0.07%, Fe: 0.7%, Cu: 0.17%, Zn: 0.03%, Ti: 0.02%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0072] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 50% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 50%), and the thickness of the high-strength and high-elongation aluminum foil is 0.4% of the intermediate annealing thickness (equivalent to a thickness difference of 99.6%).
[0073] Example 6
[0074] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 5.8 μm, and the rolling texture of the aluminum foil accounts for 57%.
[0075] Aluminum foil includes the following components by mass percentage:
[0076] Si: 0.03%, Fe: 0.7%, Cu: 0.22%, Zn: 0.03%, Ti: 0.025%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0077] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 49% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 51%), and the thickness of the high-strength and high-elongation aluminum foil is 5% of the intermediate annealing thickness (equivalent to a thickness difference of 95%).
[0078] Example 7
[0079] A high-strength and high-elongation aluminum foil, the preparation method of which comprises steps substantially the same as those of Example 1, the difference being that the intermediate annealing temperature is 320° C. and the time is 8 hours.
[0080] Example 8
[0081] A high-strength and high-elongation aluminum foil, the preparation method of which comprises steps substantially the same as those of Example 1, the difference being that the intermediate annealing is performed at a temperature of 300° C. and for a time of 8 hours.
[0082] Example 9
[0083] A high-strength and high-elongation aluminum foil, the preparation method of which comprises steps substantially the same as those of Example 1, the difference being that the intermediate annealing temperature is 450° C. and the time is 4 hours.
[0084] Example 10
[0085] A high-strength and high-elongation aluminum foil, the preparation method of which comprises the same steps as those in Example 1, except that the heating rate of the intermediate annealing from room temperature to the required annealing temperature is 50°C / h.
[0086] Comparative Example 1
[0087] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 6.8 μm, and the rolling texture of the aluminum foil accounts for 68%.
[0088] Aluminum foil includes the following components by mass percentage:
[0089] Si: 0.06%, Fe: 0.58%, Cu: 0.15%, Zn: 0.03%, Ti: 0.018%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0090] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 62% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 38%), and the thickness of the high-strength and high-elongation aluminum foil is 0.9% of the intermediate annealing thickness (equivalent to a thickness difference of 99.1%).
[0091] Comparative Example 2
[0092] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.1 μm, and the rolling texture of the aluminum foil accounts for 78%.
[0093] Aluminum foil includes the following components by mass percentage:
[0094] Si: 0.08%, Fe: 0.65%, Cu: 0.19%, Zn: 0.02%, Ti: 0.023%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0095] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 35% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 65%), and the thickness of the high-strength and high-elongation aluminum foil is 1.2% of the intermediate annealing thickness (equivalent to a thickness difference of 98.8%).
[0096] Comparative Example 3
[0097] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 5.8 μm, and the rolling texture of the aluminum foil accounts for 50%.
[0098] Aluminum foil includes the following components by mass percentage:
[0099] Si: 0.09%, Fe: 0.52%, Cu: 0.09%, Zn: 0.03%, Ti: 0.015%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0100] The preparation method of the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 52% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 48%), and the thickness of the high-strength and high-elongation aluminum foil is 7% of the intermediate annealing thickness (equivalent to a thickness difference of 93%).
[0101] Comparative Example 4
[0102] A high-strength and high-elongation aluminum foil. Through EBSD detection, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 3.6 μm, and the rolling texture of the aluminum foil accounts for 81%.
[0103] Aluminum foil includes the following components by mass percentage:
[0104] Si: 0.075%, Fe: 0.6%, Cu: 0.1%, Zn: 0.03%, Ti: 0.019%, other single impurity elements ≤ 0.05%, the balance is aluminum;
[0105] The method for preparing the high-strength and high-elongation aluminum foil comprises the steps basically the same as those in Example 1, with the difference that the intermediate annealing thickness is 47% of the thickness of the cast-rolled coil (equivalent to a thickness difference of 53%), and the thickness of the high-strength and high-elongation aluminum foil is 0.3% of the intermediate annealing thickness (equivalent to a thickness difference of 99.7%).
[0106] The average grain size of the surface layer annealing, the average grain size of the middle cross section annealing and the average grain size of the middle longitudinal section annealing in Examples 1 to 6 and Comparative Examples 1 to 4 are measured and are shown in Table 1.
[0107] Table 1
[0108]
[0109] Depend on Figure 1 It can be seen that the surface annealed grain structure is uniform, and the average grain size is 155μm; Figure 2 and Figure 3 It can be seen that the annealed grain structure in the middle cross section is uniform, and the average grain size is 77 μm. Figure 4 and Figure 5 It can be found that the annealed grain structure in the middle longitudinal section is uniform and the average grain size is 73 μm.
[0110] At the same time by Figure 6 and Figure 7 It can be seen that the grain size of aluminum foil is ≤6μm; Figure 8 and Fig. 9 It can be found that the rolling texture of aluminum foil accounts for 55% to 76%.
[0111] Results
[0112] The strength and elongation of high-strength and high-elongation aluminum foil are tested using P7 test in GB / T228.1, with a tensile speed of 3 mm / min and a gauge length of 50 mm. The test structure is shown in Table 2.
[0113] Table 2
[0114]
[0115] It can be seen from the test results in Table 2 above that the aluminum foil strength of the high-strength and high-elongation aluminum foil in Examples 1 to 6 can reach 256 to 277 MPa, and the elongation can reach 4.3% to 4.9%, which can fully meet the performance requirements of aluminum foil for lithium battery current collectors.
[0116] In Comparative Example 1, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 6.8 μm, the grain size is too large, and the final strength of the aluminum foil is low; in Comparative Example 2, the rolling texture of the aluminum foil with a thickness of 0.010-0.020 mm accounts for 78%, the rolling texture accounts for too large a proportion, and the final elongation of the aluminum foil is low.
[0117] In Comparative Example 3, the grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 5.8 μm, and the rolling texture of the aluminum foil accounts for 50%. The rolling texture accounts for too small a proportion, and the strength and elongation of the aluminum foil are significantly reduced.
[0118] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A high-strength and high-elongation aluminum foil, characterized in that: Through EBSD testing, it was determined that the grain size of aluminum foil with a thickness of 0.010-0.020 mm was ≤6 μm, and the rolling texture of the aluminum foil accounted for 55%-76%; The aluminum foil is composed of the following components by mass percentage: composition: Si: 0.03%~0.09%, Fe: 0.52%~0.7%, Cu: 0.09%~0.22%, Zn≤0.03%, Ti: 0.015%~0.025%, other single impurity elements ≤0.05%, the balance is aluminum; The aluminum foil is prepared by a casting and rolling method, which comprises the following steps: First, the aluminum foil raw material is successively smelted and cast-rolled to form a cast-rolled coil; The cast rolled coil is then subjected to cold rolling, intermediate annealing and foil rolling in sequence to obtain high-strength and high-elongation aluminum foil; The thickness of the intermediate annealing is 40% to 59% of the thickness of the cast-rolled coil, and the thickness of the high-strength and high-elongation aluminum foil is 0.4% to 5% of the thickness of the intermediate annealing.
2. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The grain size of the aluminum foil with a thickness of 0.010-0.020 mm is 4.5-5.6 μm.
3. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The rolling texture of the aluminum foil accounts for 60% to 75%.
4. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The thickness of the intermediate annealing is 45% to 55% of the thickness of the cast-rolled coil.
5. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The thickness of the high-strength and high-elongation aluminum foil is 0.4% to 2% of the intermediate annealing thickness.
6. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The grain structure of the surface, cross section and longitudinal section after intermediate annealing is uniform, and the average grain size on the surface is 100~300μm; The average grain size in the cross section is ≤100μm; the average grain size in the longitudinal section is ≤100μm.
7. The high-strength and high-elongation aluminum foil according to claim 6, characterized in that: The grain structure of the surface, cross section and longitudinal section after intermediate annealing is uniform, and the average grain size on the surface is 100~200μm; The average grain size in the cross section is 70~95μm; the average grain size in the longitudinal section is 70~95μm.
8. The high-strength and high-elongation aluminum foil according to claim 1, characterized in that: The intermediate annealing temperature is 300-450° C., the holding time is 4-8 hours, and the heating rate from room temperature to the required annealing temperature is ≥40° C. / h.
9. The high-strength and high-elongation aluminum foil according to claim 8, characterized in that: The intermediate annealing temperature is 320-400° C., the holding time is 4-8 hours, and the heating rate from room temperature to the required annealing temperature is ≥50° C. / h.
10. Use of the high-strength and high-elongation aluminum foil according to any one of claims 1 to 9 in a lithium-ion battery.
Citation Information
Patent Citations
Aluminum foil for 1N00 lithium battery and preparation method of aluminum foil
CN113564425A
Aluminium foil
WO1995025825A1