A kind of wide temperature type electrolytic capacitor paper and preparation method thereof
By using electrolytic capacitor paper with nanofiber and fibrils combined in electrolytic capacitor paper, and adding antifreeze, high-temperature stabilizer and hydrogen dehydrating agent to its coating layer, the aluminum electrolytic capacitor is solved in extremely cold and high-temperature environments. The performance attenuation problem achieves stable performance and prolong service life in a wide temperature range.
Patent Information
- Application Number
- CN202211614801.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-15
AI Technical Summary
Existing aluminum electrolytic capacitors show problems such as increasing impedance, attenuation of capacity and leakage current in extremely low and high temperature environments, which is difficult to meet the needs of extremely cold environments such as new energy vehicles and communication base stations.
Using electrolytic capacitor paper composed of nanofibers and fibres, and adding antifreeze, high-temperature stabilizer and hydrogen dehydrating agent to its coating layer, it is prepared by a double-layer composite molding process to form a suitable pore structure to improve the electrolyte. fluidity and pressure resistance.
The normal performance of the capacitor can be maintained in the environment of -55℃ and 125℃, reducing the equivalent series resistance value and leakage current, and extending the service life of the capacitor.
Smart Images

Figure BDA0004000109900000081 
Figure BDA0004000109900000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of capacitor paper, and in particular relates to a wide-temperature electrolytic capacitor paper and a preparation method thereof. Background Art
[0002] The current operating environment temperature of aluminum electrolytic capacitors is in the range of -40℃ to 105℃. When the temperature is lower than -40℃, the electrolyte freezes at low temperature, the impedance of the capacitor increases sharply, and the capacity decays sharply. The capacity decay can reach more than 50%, and the reliability is greatly reduced. It is difficult to meet the requirements of new energy vehicles, charging piles, communication base stations, etc. for extremely cold environments (-55℃), which seriously limits the application of aluminum electrolytic capacitors in extremely low temperature environments. When the operating temperature exceeds 105℃, the leakage current of the capacitor increases sharply, the ripple resistance decreases rapidly, and the air pressure in the aluminum shell increases, affecting the use characteristics and life of the capacitor, and even causing explosion and failure. Therefore, it is urgent to develop an electrolytic capacitor paper that can function normally in both low and high temperature working environments to meet the needs of aluminum electrolytic capacitor use conditions.
[0003] Chinese invention patent CN114649148A discloses a production process of a low-temperature resistant aluminum electrolytic capacitor working electrolyte. The electrolyte raw materials include 55-70 parts of the main solvent, 10-15 parts of the auxiliary solvent, 8-16 parts of the solute, 2-8 parts of the pH regulator, 1-4 parts of the dehydrogenation agent, 1-2 parts of the water blocking agent, the main solvent is water and ethylene glycol, the auxiliary solvent includes any one of N-methylformamide or 3-methylcyclobutane sulfone, and the solute is any one or two of ammonium hydrogen azelaic acid, 1,5-dodecanedioic acid, butyl phosphate and terephthalic acid. The low-temperature resistance of the electrolyte can be improved by using a solvent with a low saturated vapor pressure, and it has good antifreeze properties. On the basis of high-temperature resistance, the low-temperature resistance is improved to achieve wide temperature use of the electrolyte. The above patents achieve wide temperature use of the electrolyte by adding various substances to the electrolyte, but they do not disclose the specific temperature range in which it can be used. Moreover, adding both high-temperature resistant and low-temperature resistant substances to the electrolyte will make the electrolyte insufficiently soluble and affect the effect of the electrolyte. Summary of the invention
[0004] In order to overcome the technical problem in the prior art that capacitors cannot function normally under high and low temperature conditions, the present invention provides a wide-temperature electrolytic capacitor paper and a preparation method thereof to enhance the antifreeze ability and high temperature resistance of the electrolytic capacitor system.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A first aspect of the present invention provides a wide temperature range electrolytic capacitor paper, the electrolytic capacitor paper comprising a fiber layer and a coating layer, the coating layer being arranged on one side or both sides of the fiber layer; the fiber layer comprising nanofibers and fibrillated fibers, the coating layer comprising an antifreeze agent, a high temperature stabilizer and a dehydrogenating agent.
[0007] The capacitor paper in the present application includes a fiber layer and a coating layer. By arranging a coating layer including an antifreeze agent, a high temperature stabilizer and a dehydrogenating agent on the fiber layer, the prepared capacitor can be used normally under high and low temperature conditions, avoiding the problem of reduced electrolyte solubility caused by adding the above substances to the electrolyte system of the electrolytic capacitor. By coating, high temperature resistance and low temperature resistance can be achieved in the same electrolytic capacitor at the same time without affecting other properties of the electrolytic capacitor. The nanofibers and fibrillated chemical fibers used in the present invention are used in combination because the shapes of the two are close to cylindrical, the fiber overlap is relatively loose, the pore structure formed is relatively rich, the liquid absorption performance is excellent, the ion passage channel is increased, and the appropriate pore structure is obtained by limiting the mass ratio of the two fibers, reducing the effect of the curvature of the diaphragm hole, and then reducing the equivalent series resistance (ESR) value of the capacitor paper. By coating the antifreeze agent on the fiber layer, the fluidity of the electrolyte in a low temperature environment can be improved, ensuring that the resistance to the migration of electrolyte ions in the system under low temperature conditions is at a relatively low level.
[0008] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the mass ratio of the nanofibers to the fibrillated fibers is (2-8):(2-8), and the mass ratio of the antifreeze agent, the high temperature stabilizer and the dehydrogenating agent is (3-7):(3-7):(1-5).
[0009] In the present invention, the mass ratio of nanofiber to fibrillated fiber is (2-8): (2-8), which can ensure that the pore size, tensile strength and other indicators of capacitor paper are within the product performance requirements. The mass ratio of antifreeze agent, high temperature stabilizer and dehydrogenating agent is (3-7): (3-7): (1-5), which can ensure that the capacitor paper can function under the environment of -55°C and 125°C.
[0010] As an optional implementation, in the electrolytic capacitor paper provided by the present invention, the antifreeze agent consists of lower alcohols, glycol monomethyl ether compounds and ammonium sebacate compounds.
[0011] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the lower alcohol includes ethylene glycol or propylene glycol, the glycol monomethyl ether compound includes diethylene glycol monomethyl ether or triethylene glycol monomethyl ether, and the ammonium sebacate compound includes ammonium sebacate or ammonium isosebacate.
[0012] In the present invention, ethylene glycol and glycerol are proton polar solvents, which have excellent solubility for organic carboxylic acid ammonium salts. The use of ethylene glycol and glycerol is that the electrolyte of the electrolyte generally contains organic carboxylic acid ammonium salts, and the capacitor paper contains components with excellent solubility for organic carboxylic acid ammonium salts, which is more conducive to the diffusion of electrolyte in the capacitor paper.
[0013] In the present invention, the freezing points of diethylene glycol monomethyl ether and triethylene glycol monomethyl ether are very low, wherein the freezing point of diethylene glycol monomethyl ether is -70°C, and the freezing point of triethylene glycol monomethyl ether is -44°C; the esterification of ammonium sebacate and isosebacic acid with ethylene glycol is small, which can improve the conductivity and antifreeze properties to a certain extent. The reason is that ester substances with high saturation are easy to crystallize and precipitate at low temperatures, causing turbidity and flocculation of the electrolyte. Small esterification can reduce the formation of ester substances with high melting points, ensuring that the electrolyte still has good fluidity at a lower temperature.
[0014] After mixing one or more of the above antifreeze agents, high and low temperatures can be complemented, thereby reducing the freezing temperature of the electrolyte. In addition, because ether solvents have a high solvation effect on ammonium cations, the activity of cations is inhibited, thereby increasing the withstand voltage of the electrolyte. After mixing the above ingredients, the electrolytic capacitor can work at a low temperature of -55°C and withstand high voltage.
[0015] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the high temperature stabilizer is one or more of boric acid, phosphoric acid, ammonium phosphate, hypophosphorous acid or ammonium hypophosphite.
[0016] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the hydrogen remover is one or more of p-nitrobenzyl alcohol, o-nitroanisole, p-nitrophenol, p-nitrophenol, and m-nitroacetophenone.
[0017] The function of the hydrogen remover in the present invention is to eliminate hydrogen generated by the electrolyte and reduce the internal pressure of the capacitor.
[0018] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the total amount of the antifreeze agent, high temperature stabilizer and hydrogen remover added is 0.5-10% of the mass of the nanofibers and fibrillated fibers.
[0019] In the present invention, the addition amount of the antifreeze agent, the high temperature stabilizer and the dehydrogenating agent is controlled within the above range, which can ensure that the capacitor paper can function under the environment of -55°C and 125°C, and will not affect other properties of the capacitor paper.
[0020] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the nanofibers include nanocellulose fibers, artificial spider silk fibers, nanobacterial cellulose fibers, nanocarbon fibers, nanoglass fibers, nanoceramic fibers, nanoalumina fibers and the like.
[0021] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the nanofiber diameter is less than 1000nm and the length is greater than 300μm. If the nanofiber length is less than 300μm, the strength of the paper is too low, affecting the application performance of the capacitor paper.
[0022] As an optional implementation, in the electrolytic capacitor paper provided by the present invention, the nanofibers have a diameter less than 500-1000 nm and a length greater than 0.7-3 mm.
[0023] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the fibrillated fibers refer to short-cut fibers that have been fibrillated, selected from one or more of polyphenylene sulfide fibers, Tencel fibers, poly(p-phenylene benzobisoxazole) fibers, poly(p-phenylene terephthalamide) fibers and poly(arylene oxadiazole) fibers, and the short-cut fibers have a length of 3 to 10 mm and an initial fineness of 0.1 to 3 dtex.
[0024] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the beating degree of the fibrillated fibers is 20 to 90° SR, and the average length is 0.1 to 3.0 mm.
[0025] The fibrillation treatment in the present invention refers to the processes of debonding, beating and refining. The fibrillated fibers refer to the fibers obtained after the short-cut fibers are treated as above. If the selected fibers need to be fibrillated, the diameter of the untreated fibers is large, the paper formed has many defects, and the interweaving bonding force between the fibers is weak, and the strength is particularly low. During the treatment process, the beating degree and length are controlled within this range, which can ensure that the capacitor paper obtained has good uniformity and strength, and at the same time ensure that the pores of the capacitor paper are not too large to cause insufficient breakdown resistance.
[0026] As an optional embodiment, in the electrolytic capacitor paper provided by the present invention, the beating degree of the fibrillated fibers is 50 to 90° and the average SR length is 0.5 to 1.5 mm.
[0027] The second aspect of the present invention provides a method for preparing the above-mentioned wide temperature type electrolytic capacitor paper, comprising the following steps:
[0028] S1, stirring and uniformly dispersing the nanofibers to obtain slurry A, and refining the chopped fibers to obtain slurry B;
[0029] S2, slurry A and slurry B are mixed uniformly according to the proportion to obtain slurry C;
[0030] S3. The slurry C is passed through a paper forming device using a double-layer composite forming method, and after pressing, drying, and rolling, a basic room temperature capacitor paper is obtained. A mixture containing an antifreeze agent, a high temperature stabilizer, and a dehydrogenating agent is coated or sprayed on one or both sides of the room temperature capacitor paper to obtain a wide temperature electrolytic capacitor paper.
[0031] A third aspect of the present invention provides the use of the wide temperature range electrolytic capacitor paper as a diaphragm material in the preparation of capacitors or lithium ion batteries.
[0032] As an optional implementation, in the application provided by the present invention, the capacitor includes a carbonization-free solid capacitor, a semi-solid capacitor or a supercapacitor.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The electrolytic capacitor paper prepared in the present invention pre-coats the compound containing antifreeze agent, high temperature stabilizer and dehydrogenating agent on the fiber layer, which can effectively solve the problem of affecting the normal function of the capacitor caused by the low solubility of the above substances in the electrolyte system of aluminum electrolytic capacitors, enhance the antifreeze ability and high temperature resistance of the electrolytic capacitor system, so that under high temperature conditions, the leakage current of the capacitor is sharply reduced, the ESR value under low temperature conditions is reduced, and the capacity attenuation is smaller. At the same time, the combination of fibrillated fibers and nanofibers is used to effectively improve the pore structure of the electrolytic capacitor paper, reduce the ESR value of the paper, and improve the tensile strength of the paper, so that the paper still shows good performance at lower temperatures. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in combination with the contents of the specification and preferred embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.
[0036] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0038] Example 1
[0039] Cellulose nanofibers with a diameter of 700nm and a length of 1.5mm are evenly dispersed to obtain pulp A; Tencel short-cut fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain pulp B by refining to 70°SR; A and B are evenly mixed in a ratio of 6:4 to obtain mixed pulp C; Mixed pulp C is made using a rotary paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 4:4:2 is evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0040] In order to test the performance of the prepared electrolytic capacitor paper, the capacitor paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0041] Example 2
[0042] Nano ceramic fibers with a diameter of 800nm and a length of 1.0mm are evenly dispersed to obtain slurry A; Tencel short-cut fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain slurry B by grinding to 85°SR; A and B are evenly mixed in a ratio of 6:4 to obtain mixed slurry C; Mixed slurry C is made using a rotary paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, phosphoric acid and p-nitrophenol in a mass ratio of 5:3:2 is evenly applied to the surface of the paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0043] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0044] Example 3
[0045] Cellulose nanofibers with a diameter of 700nm and a length of 1.5mm are evenly dispersed to obtain pulp A; poly(p-phenylene terephthalamide) fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain pulp B by refining to 85°SR; the two pulps A and B are evenly mixed in a ratio of 6:4 to obtain mixed pulp C; the mixed pulp C is made by a rotary paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 5:3:2 is evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0046] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0047] Example 4
[0048] Nano ceramic fibers with a diameter of 800nm and a length of 1.0mm are uniformly dispersed to obtain slurry A; poly(p-phenylene terephthalamide) fibers with a length of 5mm and a fineness of 1.7dtex and tencel short-cut fibers are used in a mass ratio of 1:1, and the slurry B is obtained by grinding to 85°SR; the two slurries A and B are uniformly mixed in a ratio of 6:4 to obtain mixed slurry C; the mixed slurry C is made by a round-net paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 3:3:4 is uniformly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0049] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0050] Example 5
[0051] Cellulose nanofibers with a diameter of 700nm and a length of 1.5mm are evenly dispersed to obtain pulp A; Tencel short-cut fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain pulp B by refining to 85°SR; A and B are evenly mixed in a ratio of 8:2 to obtain mixed pulp C; Mixed pulp C is made using a rotary paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 5:3:2 is evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0052] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0053] Example 6
[0054] Cellulose nanofibers with a diameter of 700nm and a length of 1.5mm are uniformly dispersed to obtain pulp A; Tencel short-cut fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain pulp B by refining to 85°SR; A and B are uniformly mixed in a ratio of 6:4 to obtain mixed pulp C; Mixed pulp C is made by a rotary paper machine, and a single-layer net forming method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture of antifreeze, ammonium phosphate and p-nitrophenol containing 50 parts of diethylene glycol monomethyl ether and 50 parts of triethylene glycol monomethyl ether in a mass ratio of 4:4:2 is uniformly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 0.5% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0055] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0056] Example 7
[0057] Cellulose nanofibers with a diameter of 700nm and a length of 1.5mm are evenly dispersed to obtain pulp A; Tencel short-cut fibers with a length of 5mm and a fineness of 1.7dtex are used to obtain pulp B by refining to 85°SR; A and B are evenly mixed in a ratio of 6:4 to obtain mixed pulp C; Mixed pulp C is made using a rotary paper machine, and a double-layer composite molding method is adopted. After pressing, drying, and rolling, a normal temperature type electrolytic capacitor paper is obtained, and the paper thickness is controlled to be (50±4.0)um. Finally, a mixture containing ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 4:4:2 is evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied is controlled to be 2% of the total fiber mass fraction, and a wide temperature type low ESR electrolytic capacitor paper is prepared.
[0058] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this embodiment was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0059] Comparative Example 1
[0060] Cellulose nanofibers with a length diameter of 700 nm and a length of 1.5 mm were evenly dispersed and papered on a rotary screen paper machine. A double-layer composite molding method was adopted and the paper thickness was controlled to be (50±4.0) um to prepare room temperature electrolytic capacitor paper.
[0061] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this reference example was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0062] Comparative Example 2
[0063] Cellulose nanofibers with a diameter of 700 nm and a length of 1.5 mm were evenly dispersed to obtain slurry A; Tencel short-cut fibers with a length of 5 mm and a fineness of 1.7 dtex were refined to 70°SR to obtain slurry B; Slurries A and B were evenly mixed in a ratio of 6:4 to obtain mixed slurry C; and room temperature electrolytic capacitor paper was prepared by papermaking on a rotary screen machine and adopting a double-layer composite molding method with a paper thickness controlled at (50±4.0) um.
[0064] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this reference example was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0065] Comparative Example 3
[0066] Tencel short-cut fibers with a length of 5 mm and a fineness of 1.7 dtex were refined to 70°SR by disc grinding; they were papered on a rotary screen machine and formed in a double-layer composite manner with a paper thickness controlled at (50±4.0) um to prepare room temperature electrolytic capacitor paper.
[0067] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this reference example was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0068] Comparative Example 4
[0069] Cellulose nanofibers with a length diameter of 700nm and a length of 1.5mm were evenly dispersed and papered on a rotary paper machine. A double-layer composite molding method was used, and the paper thickness was controlled to be (50±4.0)um to prepare a room temperature electrolytic capacitor paper. Finally, a mixture of ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 4:4:2 was evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied was controlled to 0.5% of the total fiber mass fraction to prepare a wide temperature type low ESR electrolytic capacitor paper.
[0070] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this reference example was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0071] Comparative Example 5
[0072] Tencel short-cut fibers with a length of 5 mm and a fineness of 1.7 dtex were refined to 70°SR by disc grinding; paper was made by a rotary paper machine, and a double-layer composite molding method was adopted. The paper thickness was controlled to (50±4.0) um to prepare normal temperature electrolytic capacitor paper. Finally, a mixture of ammonium sebacate, ammonium phosphate and p-nitrophenol in a mass ratio of 4:4:2 was evenly applied to the surface of the electrolytic capacitor paper by surface spraying, and the amount of the mixed substance applied was controlled to 0.5% of the total fiber mass fraction to prepare a wide temperature type low ESR electrolytic capacitor paper.
[0073] In order to test the performance of the prepared electrolytic paper, the electrolytic paper of this reference example was used to make a 100V aluminum electrolytic capacitor, and the components of the electrolyte included the following substances: 47.5% ethylene glycol (capacitor grade), 47.5% N,N-dimethylformamide, and 5% ammonium maleate.
[0074] 2. Performance Testing
[0075] The electrolytic capacitor papers prepared in the embodiments and comparative examples were subjected to basic performance tests, and the testing methods for the performance data were as follows: thickness testing method: GB / T451.3-.2002; tensile strength testing method: GB / T12914-2008; liquid absorption height testing: GB / T461.1-2002; ESR testing method: using Agilent bridge, model: Agilent4285A (Agilent Corporation, USA); average pore size testing method: using capillary flow pore size analyzer model: CFP-1100-A (PMI Corporation, USA), tested by bubble point method.
[0076] The test results are shown in Table 1:
[0077] Table 1: Test data of temperature rise of electrolytic container paper and capacitor prepared in Examples and Comparative Examples
[0078]
[0079]
[0080] It can be seen from Table 1 that compared with the normal temperature electrolytic capacitor paper prepared in Comparative Example 1, the wide temperature electrolytic capacitor paper prepared in Examples 1-7 has a lower ESR value and a smaller capacitance change when working in a -55°C environment, which is beneficial to improving the low temperature performance of the capacitor. It has a lower leakage current when working in a 125°C environment, which is beneficial to improving the safety and service life of the capacitor at high temperatures.
[0081] Comparative analysis of Examples 1, 2 and 3 shows that after adding fibrillated fibers, the average pore size of the paper becomes larger, the tensile strength increases, the ESR value of the capacitor becomes larger, and the high and low temperature performance becomes worse.
[0082] By comparing and analyzing Comparative Example 3 and Example 1, it can be learned that after spraying the mixed functional agent, the average pore size of the paper is smaller, the capacitance attenuation of the capacitor is smaller in an ultra-low temperature environment of -55°C, and the ESR value is smaller, and the capacitance attenuation of the capacitor is smaller in an ultra-low temperature environment of 125°C, and the ESR value is smaller.
[0083] By comparing and analyzing Examples 1 and 2, it can be seen that when the beating degree of fibrillated fibers is increased, the tensile strength of the paper is improved to a certain extent, and the average pore size is smaller; the low-temperature performance and high-temperature performance do not change much.
[0084] Through comparative analysis of Examples 2, 3 and 4, it can be seen that at the same beating degree, different fibrillated fibers have different effects on the pore size of paper.
[0085] Through comparative analysis of Examples 2 and 5, it can be seen that the more nanofibers there are, the smaller the pore size of the paper.
[0086] Through comparative analysis of Examples 2 and 6, it can be seen that the single-layer molding method and the double-layer composite molding method have no obvious effect on paper performance.
[0087] Through comparative analysis of Examples 2 and 7, it can be learned that, within the scope of the present invention, the more mixed functional agents are applied to the surface of the paper, the better the low-temperature performance and high-temperature performance of the capacitor will be.
[0088] Comparative analysis of Example 1 and Comparative Example 4 shows that when nanofibers are used alone, the tensile strength of the capacitor paper is greater. Comparative analysis of Example 5 and Comparative Example 5 shows that when chopped fibers are used alone, the average pore size of the capacitor paper is larger, both of which affect the performance of the capacitor paper.
[0089] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing a wide temperature range electrolytic capacitor paper, characterized in that: The following steps are involved: S1, stirring and uniformly dispersing the nanofibers to obtain slurry A, and refining the chopped fibers to obtain slurry B; S2, slurry A and slurry B are mixed uniformly according to the proportion to obtain slurry C; S3, the slurry C is passed through a paper forming device in a double-layer composite forming manner, and after being pressed, dried, and rolled, a basic room temperature capacitor paper is obtained, and a mixture containing an antifreeze agent, a high temperature stabilizer, and a dehydrogenating agent is sprayed on one or both sides of the room temperature capacitor paper to obtain a wide temperature electrolytic capacitor paper; The wide temperature range electrolytic capacitor paper is composed of a fiber layer and a coating layer, wherein the coating layer is arranged on one side or both sides of the fiber layer; the fiber layer is composed of nanofibers and fibrillated fibers, and the coating layer is composed of an antifreeze agent, a high temperature stabilizer and a hydrogen remover; the fibrillated fibers refer to short-cut fibers that have been fibrillated; The mass ratio of the nanofiber to the fibrillated fiber is (2-8): (2-8); the diameter of the nanofiber is 700-800nm and the length is 1-1.5mm; the beating degree of the fibrillated fiber is 70-85°SR; The mass ratio of the antifreeze agent, the high temperature stabilizer and the dehydrogenating agent is (3-7): (3-7): (1-5); the total amount of the antifreeze agent, the high temperature stabilizer and the dehydrogenating agent added is 0.5-10% of the mass of the nanofibers and the fibrillated fibers; The antifreeze agent is a mixture of diethylene glycol monomethyl ether and triethylene glycol monomethyl ether, or ammonium sebacate; The high temperature stabilizer is selected from one or more of boric acid, phosphoric acid, ammonium phosphate, hypophosphorous acid or ammonium hypophosphite; the dehydrogenating agent is selected from one or more of p-nitrobenzyl alcohol, o-nitroanisole, p-nitrophenol and m-nitroacetophenone.
2. The method for preparing wide temperature range electrolytic capacitor paper according to claim 1, characterized in that: The nanofiber is selected from one or more of nanocellulose fiber, artificial spider silk fiber, nano bacterial cellulose fiber, nano carbon fiber, nano glass fiber, nano ceramic fiber and nano alumina fiber.
3. The method for preparing wide temperature range electrolytic capacitor paper according to claim 1, characterized in that: The chopped fibers are selected from one or more of polyphenylene sulfide fibers, tencel fibers, poly(p-phenylene benzobisoxazole) fibers, poly(p-phenylene terephthalamide) fibers and poly(arylene oxadiazole) fibers. The chopped fibers have a length of 3-10 mm and an initial fineness of 0.1-3 dtex.
4. The method for preparing wide temperature range electrolytic capacitor paper according to claim 1, characterized in that: The average length of the fibrillated fibers is 0.1-3.0 mm.
5. Use of the wide temperature range electrolytic capacitor paper prepared by the method for preparing the wide temperature range electrolytic capacitor paper according to any one of claims 1 to 4 as a diaphragm material in preparing capacitors or lithium ion batteries.
6. The use according to claim 5, characterized in that: The capacitor includes a carbonization-free solid capacitor, a semi-solid capacitor or a supercapacitor.
Citation Information
Patent Citations
Production process of working electrolyte of low-temperature-resistant aluminum electrolytic capacitor
CN114649148A
A 600V high-voltage high-temperature resistant long-life aluminum electrolytic capacitor and a manufacturing method thereof
CN109192509A
Coating-enhanced carbonization-free solid electrolytic capacitor paper and preparation method thereof
CN109235137A
Carbonization-free diaphragm paper as well as preparation method and application thereof