An early-strength gelling material based on partially calcined hydromagnesite and a preparation method thereof
Preparation of early-strength gelling materials by combining partially calcined water magnesite with ore powder has been solved, and the performance of low reaction activity of calcined products has been improved, which has achieved low energy consumption and high added value-added gelling materials, significantly improved early strength and expanded The use of low-grade water magnesite is achieved.
Patent Information
- Application Number
- CN202310166552.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-24
AI Technical Summary
In the prior art, the low reactive activity of magnesite calcined products affects the performance of gelled materials, especially early strength development and volume stability.
Partially calcined water magnesite and ore powder are used to prepare early-strength gelling materials, and a mixture containing magnesium oxide and amorphous magnesium carbonate is formed by low-temperature calcination, which promotes hydration of magnesium oxide, forms Mg(OH)2 and forms M- (A)-S-H gel and hydrotalcite to improve early strength.
It reduces energy consumption and costs, improves the utilization rate of low-grade water magnesite, significantly improves early strength and continuously provides strength development, avoiding the impact of decomposition of calcium ores on the hydration process.
Smart Images

Figure CN116199486B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to an early-strength gelling material based on partially calcined hydromagnesite and a preparation method thereof. Background Art
[0002] my country has rich reserves of hydromagnesite. In the Bange Lake area of Tibet alone, the reserves of hydromagnesite are more than 100 million tons, which is a large-scale deposit with important industrial development value. Existing research shows that hydromagnesite is an ideal natural mineral raw material for the preparation of magnesium products such as flame retardants, magnesium oxide, heavy / light basic magnesium carbonate, magnesium hydroxide, etc. It is environmentally friendly, rich in resources, low in cost, and cost-effective. However, due to factors such as geography, transportation, and technology, its development and utilization are limited. Therefore, how to develop and utilize hydromagnesite is the main research and development work at present.
[0003] Cement is one of the most widely used building materials in the world. However, the cement industry causes a large amount of carbon dioxide emissions every year, which is not conducive to the protection of the ecological environment and sustainable development. Compared with silicate cement with similar compressive strength grades, the use of magnesium-based hydraulic cementitious materials is considered to be one of the most effective measures to reduce carbon dioxide emissions. Studies have shown that magnesium oxide can stimulate various auxiliary cementitious materials, such as metakaolin, mineral powder, silica fume, fly ash, etc., and its stimulation effect mainly depends on the activity of magnesium oxide. In the actual production of commercial reactive MgO, in order to improve the purity of MgO, magnesite (hydromagnesite) is often calcined at least 2h at a temperature not lower than 800℃ to ensure that it is completely decomposed into MgO. However, higher calcination temperatures and longer holding times will increase the degree of crystallization of MgO, thereby reducing its reactivity. The low reactivity of MgO is not only not conducive to the early strength development of cementitious materials, but also the hydration of unreacted MgO in the later stage will affect the volume stability of cementitious materials.
[0004] In addition, calcium and magnesium ores often coexist in nature. High-temperature calcination will not only decompose hydromagnesite into MgO, but also cause calcium ores (dolomite, limestone, etc.) to decompose into CaO. The hydration of CaO will consume additional water and release a large amount of heat, seriously affecting the hydration process of magnesium-based cementitious materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, propose an early-strength cementitious material based on partially calcined hydromagnesite and a preparation method thereof, and solve the technical problem in the prior art that the low reaction activity of the calcined product of hydromagnesite affects the performance of the cementitious material.
[0006] In a first aspect, the present invention provides an early-strength cementitious material based on partially calcined hydromagnesite, the raw materials of which include: partially calcined hydromagnesite and mineral powder; wherein the composition of the partially calcined hydromagnesite includes: amorphous magnesium carbonate, magnesium oxide and inevitable impurities.
[0007] In a second aspect, the present invention provides a method for preparing the above-mentioned early-strength cementitious material based on partially calcined hydromagnesite, comprising the following steps:
[0008] The partially calcined hydromagnesite, mineral powder, water reducer and water are uniformly mixed, then poured into a mold, and after demoulding and curing, an early strength cementitious material based on the partially calcined hydromagnesite is obtained.
[0009] Compared with the prior art, the beneficial effects of the present invention include:
[0010] Compared with completely calcined hydromagnesite, the partially calcined hydromagnesite of the present invention has a lower calcination temperature, a shorter insulation time, lower energy consumption, lower cost, and a simple process flow. In addition, low-grade hydromagnesite can be used for calcination, and only the raw materials need to be ground and screened without the need for chemical reagents. This reduces energy consumption while increasing the utilization rate of low-grade hydromagnesite, and is a sustainable material with high added value and environmental friendliness. The present invention prepares a cementitious material by compounding partially calcined hydromagnesite with mineral powder. The amorphous magnesium carbonate formed by the partial calcination can accelerate the hydration of magnesium oxide, promote the large-scale formation of Mg(OH)2 at the initial stage of hydration, and refine the pore structure, thereby greatly improving the early strength. The active silica-alumina in the mineral powder reacts in the alkaline environment provided by the Mg(OH)2 formed by hydration to generate products such as M-(A)-SH gel and hydrotalcite, thereby continuously providing strength development. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 The 3h and 1d compressive strengths of the early strength gelling materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2 of the present invention;
[0012] Figure 2 is the XRD pattern of the partially calcined hydromagnesite powder used in Examples 1 to 3 of the present invention;
[0013] Figure 3 It is the infrared spectrum of the partially calcined hydromagnesite powder used in Examples 1 to 3 of the present invention, the completely calcined hydromagnesite powder used in Comparative Example 1, and the analytically pure MgO used in Comparative Example 2. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0015] In a first aspect, the present invention provides an early-strength cementitious material based on partially calcined hydromagnesite, the raw materials of which include: partially calcined hydromagnesite and mineral powder; wherein the composition of the partially calcined hydromagnesite includes: amorphous magnesium carbonate, magnesium oxide and inevitable impurities.
[0016] The present invention forms a mixture containing magnesium oxide and amorphous magnesium carbonate by partially calcining hydromagnesite at low temperature, and accelerates the hydration of magnesium oxide through the nucleation effect of trihydrate magnesite (MgCO3·3H2O), a hydration product of amorphous magnesium carbonate, thereby indirectly improving the hydration activity of magnesium oxide, promoting the formation of Mg(OH)2 at the initial stage of hydration, and greatly improving the early strength of the system. In addition, under the alkaline environment provided by Mg(OH)2, active siliceous and aluminumous substances in the mineral powder are dissolved and form products such as M-(A)-SH gel and hydrotalcite, so that the system has continuous strength development. The present invention does not require the addition of external chemical reagents and high-temperature calcination, and at the same time expands the utilization of low-grade hydromagnesite, and has high application value and social and economic benefits.
[0017] Preferably, the content of magnesium oxide in the above-mentioned partially calcined hydromagnesite is 50% to 95%, more preferably 50% to 85%. The decomposition of hydromagnesite (4MgCO3·Mg(OH)2·4H2O) is divided into three processes: loss of bound water, dehydroxylation and decarburization. The temperature ranges in which the three processes occur overlap. In order to calcine a mixture of MgO and amorphous MgCO3, at least the hydroxyl group in Mg(OH)2 needs to be removed, and when this decomposition process occurs, amorphous MgCO3 is also decomposed. The inventors conducted XRD analysis on the powders obtained under different calcination systems and found that in the powders where the MgO diffraction peak just appeared, the MgO content was already more than 50%, and the powders obtained at lower calcination temperatures had no MgO diffraction peaks, and only showed some characteristic peaks of hydromagnesite, and the product was still in the 4MgCO3·Mg(OH)2 stage. Therefore, if one wants to calcine a product with a lower MgO content, its composition is not a binary mixture of MgO and amorphous magnesium carbonate, but 4MgCO3·Mg(OH)2.
[0018] In some specific embodiments of the present invention, the preparation step of the partially calcined hydromagnesite includes: calcining the ground and sieved hydromagnesite to obtain partially calcined hydromagnesite; wherein the mesh size of the sieve is 200 mesh; the heating rate is: room temperature to 200°C, 3 to 6°C / min; 200°C to a specified calcination temperature, 8 to 12°C / min; the calcination temperature is 400°C to 600°C, and the insulation time is 60min to 120min; or, the calcination temperature is 600°C to 700°C, and the insulation time is 0min to 60min.
[0019] Preferably, the 4MgCO3·Mg(OH)2·4H2O content in the above hydromagnesite is ≥70%, and the Fe2O3 content is ≤2.0%. The inventors found in preliminary experiments that when low-grade hydromagnesite (4MgCO3·Mg(OH)2·4H2O content is about 75%, and Fe2O3 content is greater than 2.5%), the powder of the hydromagnesite with a higher Fe content is light yellow after calcination, and gradually turns into reddish brown as the calcination temperature increases, and the effect of stimulating the mineral admixture is greatly reduced. It can be seen that the Fe2O3 content in the hydromagnesite has a great influence on the performance of the early-strength cementitious material. In order to obtain an early-strength cementitious material with better performance, the Fe2O3 content needs to be controlled to be ≤2%.
[0020] More preferably, the content of 4MgCO3·Mg(OH)2·4H2O is ≥90%, and the content of Fe2O3 is ≤1%.
[0021] Preferably, the activity grade of the mineral powder is S95 or S105.
[0022] Preferably, the mass ratio of magnesium oxide to mineral powder in the partially calcined hydromagnesite is 1:(2-6). Within this mass ratio range, the formed early-strength gelling material has the highest compressive strength.
[0023] More preferably, the mass ratio of magnesium oxide to mineral powder in the partially calcined hydromagnesite is 1:5.
[0024] Preferably, the raw materials of the above-mentioned early-strength cementitious material based on partially calcined hydromagnesite also include: a water reducing agent and water.
[0025] In some specific embodiments of the present invention, the water reducer is a polycarboxylate water reducer.
[0026] Furthermore, the water reducing agent accounts for 0.5% to 1.5% of the total mass of the calcined hydromagnesite and the mineral powder, and further 1.0%; water accounts for 35% to 50% of the total mass of the calcined hydromagnesite and the mineral powder, and further 40%.
[0027] Preferably, the raw materials of the above-mentioned early-strength cementitious material based on partially calcined hydromagnesite do not include cement clinker.
[0028] In a second aspect, the present invention provides a method for preparing the above-mentioned early-strength cementitious material based on partially calcined hydromagnesite, comprising the following steps:
[0029] The partially calcined hydromagnesite, mineral powder, water reducer and water are uniformly mixed, then poured into a mold, and after demoulding and curing, an early strength cementitious material based on the partially calcined hydromagnesite is obtained.
[0030] Preferably, demoulding is performed after standing for 1 day.
[0031] The present invention does not limit the curing time, and those skilled in the art can select it according to actual conditions. For example, the curing time can be ≥3h.
[0032] In some specific embodiments of the present invention, the step of uniformly mixing the partially calcined hydromagnesite, mineral powder, water reducing agent and water is specifically as follows:
[0033] Mix part of the calcined hydromagnesite and the mineral powder in a mixer for 60 seconds;
[0034] Add water and part of the water reducing agent into the mixer and mix for 60 seconds;
[0035] Add the remaining water reducing agent into the mixer and mix for 60 to 120 seconds to obtain a mixture.
[0036] To avoid redundancy, in the following embodiments and comparative examples of the present invention, unless otherwise specified, the preparation method of the clinker-free early-strength cementitious material based on partially calcined hydromagnesite is as follows:
[0037] (1) grinding the hydromagnesite to pass a 200-mesh sieve, partially calcining the hydromagnesite under different calcination conditions, and cooling the hydromagnesite with the furnace after the calcination to obtain partially calcined hydromagnesite;
[0038] (2) mixing part of the calcined hydromagnesite and the mineral powder in a blender for 60 seconds according to a certain proportion to obtain a gelling component;
[0039] (3) adding water and half of the water reducer to the gelling component, mixing for 60 seconds, then adding the remaining water reducer, and continuing to stir for 60 to 120 seconds to obtain a mixture;
[0040] (4) The mixture is poured into a mold, left to stand for 1 day, and then demolded and cured to obtain an early-strength cementitious material based on partially calcined hydromagnesite.
[0041] The content of 4MgCO3·Mg(OH)2·4H2O in the hydromagnesite used is 92.08%, and the content of Fe2O3 is 0.83%; the activity grade of the mineral powder used is S95; the water reducer used is a polycarboxylate water reducer with a solid content of 60%.
[0042] The partially calcined hydromagnesite powder used in Examples 1 to 3 was first ground through a 200-mesh sieve, and then placed in a certain rotary furnace for partial calcination according to the calcination system shown in Table 1, with a heating rate of: room temperature to 200°C, 5°C / min; 200°C to the specified calcination temperature, 10°C / min. The partially calcined hydromagnesite consists of amorphous magnesium carbonate and magnesium oxide. To determine the magnesium oxide content, 20.00g of the partially calcined hydromagnesite was secondary calcined at 1000°C-3h until it was completely decomposed. According to the ignition loss of the secondary calcination, the magnesium oxide content W was calculated by the following formula: MgO(Since the CaCO3 content in hydromagnesite is less than 1.0%, its ignition loss is less than 0.5%. For the convenience of calculation, the mass loss of CaCO3 in the secondary calcination is ignored), and the results are listed in Table 1.
[0043] W MgO =1-LOI*84 / 44
[0044] Table 1 Calcination system and magnesium oxide content of partially (completely) calcined hydromagnesite powder used in Examples 1 to 3 and Comparative Example 1
[0045]
[0046]
[0047] In Examples 1 to 3, part of the calcined hydromagnesite powder is mixed with S95 grade ore powder, and the mass ratio of magnesium oxide to ore powder is controlled to be 1:5 (the part of the added calcined hydromagnesite with a mass exceeding 160.00g is identified as amorphous magnesium carbonate), the water-cement ratio is 0.4 (amorphous magnesium carbonate will also participate in hydration, and it is taken into account when calculating the water-cement ratio), and 1% of the solid mass of polycarboxylic acid water reducer is added to ensure good fluidity of the slurry. Compared with Examples 1 to 3, the difference in Comparative Example 1 is that the hydromagnesite is completely decomposed into MgO, and no amorphous magnesium carbonate is present, and the difference in Comparative Example 2 is that the added MgO is an analytically pure reagent. The specific mix ratio is shown in Table 2. Mechanical properties test The compressive strength test was carried out in accordance with GB / T17671-1999 "Test Method for Strength of Cement Mortar", and the test results are shown in Figure 1 .
[0048] Table 2 Examples and Comparative Examples Raw Material Composition (g)
[0049]
[0050] from Figure 1 It can be seen that Examples 1 to 3 have considerable compressive strength after 3 hours, and their strength increases with the increase of amorphous magnesium carbonate content; while Comparative Examples 1 to 2 have not hardened after 3 hours of hydration, and the 1d compressive strength of Examples 1 to 3 is also significantly higher than that of Comparative Examples 1 to 2, indicating that a large amount of hydration products are generated in the early stage of Examples 1 to 3 and contribute to the strength. On the one hand, it is because the magnesium oxide produced by low-temperature partial calcination has higher activity and faster reaction speed; on the other hand, although the hydration product of amorphous magnesium carbonate (magnesium carbonate trihydrate) itself has no strength and cannot stimulate the mineral powder to produce strength, the presence of amorphous magnesium carbonate further accelerates the hydration of magnesium oxide. Under the combined action of the two, magnesium oxide quickly completes the transformation to Mg(OH)2 in the early stage, expands in volume and refines the pore structure, so that Examples 1 to 3 quickly harden and have considerable early strength.
[0051] Figure 2 and Figure 3 The following are the XRD patterns and infrared spectra of partially calcined hydromagnesite powder. Figure 2 It can be seen that, in addition to a small amount of CaCO3 and SiO2 in the hydromagnesite raw material itself, only the diffraction peak of MgO appears. XRD shows that the only product of hydromagnesite calcination is MgO, and its diffraction peak gradually becomes sharper with the increase of calcination temperature and calcination time, which indicates that the crystallization degree of MgO is gradually increasing, the structure tends to be stable, and the reaction activity is gradually decreasing. However, the ignition loss of partially calcined hydromagnesite powder after secondary calcination in Table 1 shows that there are still a lot of decomposable substances in it. Figure 3 This is confirmed by the infrared spectrum of Figure 3 It can be seen that compared with Comparative Examples 1 to 2, Examples 1 to 3 have 1450 cm -1 CO3 2- Symmetric stretching vibration and 876cm -1 CO3 2- Bending vibration (there is also a weak vibration at the corresponding position in Comparative Example 1, which is the CO3 in CaCO3 2- This indicates that MgCO3 still exists in an amorphous form in the calcined powder.
[0052] In summary, the present invention obtains partially calcined hydromagnesite by keeping hydromagnesite at a relatively low temperature for a relatively short time, which is a mixture of MgO and amorphous magnesium carbonate. Low-temperature partial calcination can not only reduce the crystallinity of MgO and improve its reactivity, but also the presence of amorphous magnesium carbonate can induce the precipitation of Mg(OH)2, indirectly promoting the hydration process of MgO. Partially calcined hydromagnesite is compounded with mineral powder to prepare cementitious material, and its early strength is significantly improved compared with the fully calcined hydromagnesite-mineral powder composite system. In addition, the lower calcination temperature avoids the decomposition of calcium ore, but exists in the cementitious material system in the form of inert filler, avoiding the influence of CaO on the hydration process of cementitious material, which means that the present application has lower requirements for the purity of the hydromagnesite used (mainly referring to calcium impurities), effectively expanding the utilization of low-grade hydromagnesite, and having high application value and social and economic benefits.
[0053] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. An early strength cementitious material based on partially calcined hydromagnesite, characterized in that: The raw materials include: partially calcined hydromagnesite and mineral powder; wherein the partially calcined hydromagnesite comprises: amorphous magnesium carbonate, magnesium oxide and inevitable impurities; wherein, The partially calcined hydromagnesite is obtained by calcining the ground and sieved hydromagnesite; In the hydromagnesite, the content of 4MgCO3·Mg(OH)2·4H2O is ≥90%, and the content of Fe2O3 is ≤1%; The content of magnesium oxide in the partially calcined hydromagnesite is 50% to 95%.
2. The early strength cementitious material based on partially calcined hydromagnesite according to claim 1, characterized in that: The preparation steps of the partially calcined hydromagnesite include: calcining the ground and sieved hydromagnesite to obtain the partially calcined hydromagnesite; wherein the heating rate is: 3-6°C / min from room temperature to 200°C; 8-12°C / min from 200°C to a specified calcination temperature; the calcination temperature is 400°C to 600°C, and the insulation time is 60min to 120min; or the calcination temperature is 600°C to 700°C, and the insulation time is 0min to 60min.
3. The early strength cementitious material based on partially calcined hydromagnesite according to claim 1, characterized in that: The activity grade of the mineral powder is S95 or S105.
4. The early strength cementitious material based on partially calcined hydromagnesite according to claim 1, characterized in that: The mass ratio of magnesium oxide to mineral powder in the partially calcined hydromagnesite is 1:(2-6).
5. The early strength cementitious material based on partially calcined hydromagnesite according to claim 1, characterized in that: The raw materials of the early strength cementitious material based on partially calcined hydromagnesite also include: a water reducing agent and water.
6. The early strength cementitious material based on partially calcined hydromagnesite according to claim 1, characterized in that: The raw materials of the early-strength cementitious material based on partially calcined hydromagnesite do not include cement clinker.
7. A method for preparing an early strength gelling material based on partially calcined hydromagnesite as claimed in claim 5, characterized in that: The steps include: The partially calcined hydromagnesite, mineral powder, water reducer and water are uniformly mixed, then poured into a mold, and after demoulding and curing, an early strength cementitious material based on the partially calcined hydromagnesite is obtained.