Diamond with surface plated with silicon carbide and preparation method thereof
By mixing the gallium silicon liquid phase medium with diamond particles in a non-oxygen environment to form a uniform silicon carbide coating, the problem of poor bonding between diamond and matrix is solved, and more efficient preparation of diamond composite materials is achieved, reducing energy consumption and improving Thermal performance.
Patent Information
- Application Number
- CN202411180184.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
Poor interfacial bonding between diamond and matrix leads to rapid loss of diamond tools and low thermal performance of composite materials. The existing silicon carbide plating methods have problems such as uneven plating and high temperature.
By heat-treating the silicon gallium mixture into a liquid phase medium under a non-oxygen environment and mixing it with diamond particles at relatively low temperatures, a uniform silicon carbide coating is formed to improve the bonding of diamond and substrate.
The plating temperature and time are reduced, the graphitization of diamond is avoided, the uniformity of the silicon carbide layer and the bonding of diamond with the matrix are significantly improved, and the process efficiency and thermal performance of diamond composite materials are improved.
Smart Images

Figure HDA0005011893470000011 
Figure HDA0005011893470000012 
Figure HDA0005011893470000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond processing, and in particular relates to a diamond with silicon carbide coated on the surface and a preparation method thereof. Background Art
[0002] Diamond has the characteristics of high hardness, high strength, good wear resistance and corrosion resistance, and is widely used in the preparation of various cutting, sawing and drilling tools. Due to the poor interface bonding between diamond and other materials, diamond particles will fall off during the use of diamond tools, greatly reducing the utilization rate of diamonds, resulting in rapid wear and tear of tools and reduced processing quality.
[0003] In the field of heat dissipation, electronic devices are developing towards multifunctionality and high miniaturization. The sharp increase in power density requires electronic packaging materials to have high thermal conductivity to ensure effective heat dissipation. Diamond has excellent thermal conductivity, and the research on using it as a second phase to prepare diamond composite materials for electronic packaging materials is becoming more and more extensive. Also, because diamond has high interfacial energy with most metals, ceramics, etc., the bonding between diamond and the matrix is not strong during the application process, and it is very easy to fall off. The thermal performance of the composite material is lower than that of the component, and the thermal performance is deteriorated.
[0004] The main way to solve the above problems is to modify the diamond surface and coat the diamond surface with a thin film, which is beneficial to reduce the graphitization of diamond in high temperature environment and solve the problem of poor interface bonding between diamond and substrate, which leads to the decrease of mechanical and thermal properties.
[0005] In order to improve the interface bonding between diamond and substrate, the elements currently used for diamond surface modification are mainly Cr, Mo, W, Ti, Zr, B, Si, and all of them have certain improvements. However, there are few studies on the interface modification of diamond with silicon. Among the carbides corresponding to the currently available plating elements, silicon carbide formed by silicon and carbon atoms on the surface of diamond has the highest thermal conductivity value, and has a small thermal expansion coefficient at high temperature, which can significantly increase the interface bonding between diamond and substrate.
[0006] However, there are also technical difficulties in coating a uniform and dense layer of silicon carbide on the surface of diamond. The existing methods for coating silicon carbide mainly include magnetron sputtering and vacuum micro-evaporation, but the existing methods for coating silicon carbide have different disadvantages and limitations. The magnetron sputtering method has a small amount of single coating, the obtained film thickness is uneven, and the equipment requirements are high; the vacuum micro-evaporation method has a high coating temperature and is prone to thermal damage to diamond. The above analysis shows that the method of coating silicon carbide on the surface of diamond needs to be further improved. Summary of the invention
[0007] Based on the technical problems existing in the background technology, a diamond with silicon carbide coated on the surface and a preparation method thereof are proposed. By adding metallic gallium to make silicon present in liquid phase below the melting point, the diamond can form a uniform silicon carbide coating in the silicon gallium liquid phase medium at a relatively low temperature, thereby improving the bonding between the diamond and the substrate during the application process.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for preparing diamond with surface coated with silicon carbide, comprising the following steps:
[0010] S1. Sequentially wash the diamond with hydrochloric acid solution and sodium hydroxide solution to obtain pretreated diamond particles;
[0011] S2. heat-treating the silicon-gallium mixture in a non-oxygen environment to obtain a silicon-gallium liquid phase medium, then mixing the pre-treated diamond particles obtained in step S1 with the silicon-gallium liquid phase medium, heating and maintaining the temperature in a non-oxygen environment to perform a plating reaction, and forming a coating on the diamond surface;
[0012] S3. Place the coated diamond obtained in step S2 in a centrifuge tube with a screen and centrifuge, dry and sieve, soak with sodium hydroxide solution, wash with deionized water, dry and sieve to obtain diamond with silicon carbide coated on the surface.
[0013] According to the above scheme, in step S1, the diamond is ultrasonically cleaned with hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral; then the diamond is ultrasonically cleaned with sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pre-treated diamond particles. Preferably, the ultrasonic cleaning time is 30 to 40 minutes.
[0014] According to the above scheme, in step S1, the concentration of the hydrochloric acid solution is 10-15wt%, and the concentration of the sodium hydroxide solution is 5-15wt%.
[0015] According to the above scheme, in step S2, the process of heat treating the silicon gallium liquid phase medium is: the temperature is 1410-1450° C., and the insulation time is 5-15 minutes.
[0016] According to the above scheme, in step S2, the plating reaction conditions are: temperature is 1200-1300° C., and the insulation time is 10-30 min.
[0017] According to the above scheme, in step S2, the silicon content in the silicon-gallium liquid phase medium is 1-9 wt%.
[0018] According to the above scheme, in step S2, the mass ratio of silicon to diamond particles in the silicon-gallium liquid phase medium is 1:(10-100).
[0019] According to the above scheme, in step S2, the particle size of silicon in the silicon-gallium liquid phase medium is 1 to 3 μm.
[0020] According to the above scheme, in step S2, in the silicon-gallium liquid phase medium, the purity of metal gallium is 99.99%, and the purity of silicon is 99.99%.
[0021] According to the above scheme, in step S2, the average particle size of the diamond particles is 100-400 μm.
[0022] According to the above scheme, in step S3, the centrifugal conditions are: rotation speed 500-1000 r / min, time 5-30 min.
[0023] According to the above scheme, in step S3, the concentration of the sodium hydroxide solution is 5 to 15 wt %, and the soaking time is 6 to 15 h.
[0024] Provided is a diamond with silicon carbide coated on the surface prepared by the method.
[0025] The beneficial effects of the present invention are:
[0026] 1. The present invention provides a method for coating silicon carbide on the surface of diamond, wherein a liquid phase in which silicon and gallium are uniformly distributed is obtained at a temperature of 1410-1450° C. by controlling the ratio of silicon and gallium, and then diamond particles and the silicon gallium liquid phase medium are mixed and plated with the silicon gallium liquid phase medium using the silicon gallium liquid phase as a medium to form a silicon carbide layer on the surface of the diamond; wherein in the silicon gallium liquid phase medium, because metal gallium is in a liquid phase at high temperature, silicon can be caused to maintain a molten state below the melting point temperature, the coating temperature can be reduced to 1200-1300° C., the heat preservation time is also greatly shortened, and the silicon carbide layer can be plated in 10-30 minutes, effectively avoiding the graphitization phenomenon of diamond at high temperature and increasing the bonding of diamond and silicon carbide layer; at the same time, the present invention uses the silicon gallium liquid phase as a medium to change the traditional solid-solid reaction into a solid-liquid reaction, which is conducive to obtaining a more uniform and dense silicon carbide layer, and significantly improves the bonding of subsequent diamond as a reinforcement phase and a matrix, and has important application prospects.
[0027] 2. The process of the present invention is simple, effectively reduces the plating temperature and time of the silicon carbide layer, reduces energy consumption, improves efficiency, and has industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The XRD spectrum, surface morphology and energy spectrum of the diamond prepared in Example 1 are shown in Figure 1; wherein 1a is the XRD spectrum of diamond, Figure 1 b is the surface morphology. Figure 1 c and 1d are energy spectra.
[0029] Figure 2 The XRD spectrum, surface morphology and energy spectrum of the diamond prepared in Example 2 are shown in Figure 2a, where 2a is the XRD spectrum of diamond, Figure 2 b is the surface morphology. Figure 2 c and 2d are energy spectra.
[0030] Figure 3 The XRD spectrum, surface morphology and energy spectrum of the diamond prepared in Example 3 are shown in Figure 3a. Figure 3 b is the surface morphology. Figure 3 c and 3d are energy spectra.
[0031] Figure 4 The XRD spectrum, surface morphology and energy spectrum of the diamond prepared in Example 4 are shown in Figure 4; wherein 4a is the XRD spectrum of diamond, Figure 4 b is the surface morphology. Figure 4 c and 4d are energy spectra.
[0032] Figure 5 The XRD spectrum, surface morphology and energy spectrum of the diamond prepared in Example 5 are shown in Figure 5; 5a is the XRD spectrum of diamond, Figure 5 b is the surface morphology. Figure 5 c and 5d are energy spectra. DETAILED DESCRIPTION
[0033] The present invention is described in detail below by way of embodiments and accompanying drawings.
[0034] In the following examples, the relevant raw material indicators are: the particle size of silicon is 1 μm, and the purity is 99.99%; the purity of metal gallium is 99.99%; and the average particle size of diamond particles is 380 μm.
[0035] Example 1
[0036] A method for coating a diamond surface with silicon carbide comprises the following steps:
[0037] S1. The diamond was ultrasonically cleaned for 30 min with a 10wt% hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral, and then the diamond was ultrasonically cleaned for 30 min in a 10wt% sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles;
[0038] S2. Place a silicon-gallium mixture with a silicon content of 1 wt% in a crucible and heat it to 1450°C in a non-oxygen environment. Keep it warm for 10 minutes to obtain a silicon-gallium liquid phase medium with uniform silicon distribution; then place the diamond in the heat-treated silicon-gallium liquid phase medium at a mass ratio of silicon to diamond of 1:33 and heat it to 1200°C in a non-oxygen environment and keep it warm for 10 minutes, then cool it to form a coating on the surface of the diamond;
[0039] S3. Place the diamond with the coating on the surface in a centrifuge tube with a screen and centrifuge at 800r / min for 30min to remove the metal gallium attached to the diamond surface, dry, sieve, soak in 12wt% sodium hydroxide solution for 12h to remove excess silicon, wash with deionized water until neutral, dry and sieve to obtain diamond with silicon carbide coating on the surface. The surface of the obtained diamond is grayish white. The surface structure is determined to be SiC by XRD and energy spectrum. Figure 1 Shown are the XRD patterns, surface morphology and energy spectrum of the prepared diamond.
[0040] Example 2
[0041] A method for coating a diamond surface with silicon carbide comprises the following steps:
[0042] S1. The diamond was ultrasonically cleaned for 30 min with a 10wt% hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral, and then the diamond was ultrasonically cleaned for 30 min in a 10wt% sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles;
[0043] S2. A silicon-gallium mixture with a silicon content of 1 wt% is placed in a crucible and heated to 1450°C in a non-oxygen environment. After keeping the temperature for 10 minutes, a silicon-gallium liquid phase medium with uniform silicon distribution is obtained; then, a diamond is placed in the heat-treated silicon-gallium liquid phase medium at a mass ratio of silicon to diamond of 1:33, and the temperature is raised to 1200°C in a non-oxygen environment, and the temperature is kept for 30 minutes, and then cooled to form a coating on the surface of the diamond;
[0044] S3. Place the diamond with the coating on the surface in a centrifuge tube with a screen and centrifuge at 800r / min for 30min to remove the metal gallium attached to the diamond surface, dry, sieve, soak in 12wt% sodium hydroxide solution for 12h to remove excess silicon, wash with deionized water until neutral, dry and sieve to obtain diamond with silicon carbide coating on the surface. The surface of the obtained diamond is grayish white. The surface structure is determined to be SiC by XRD and energy spectrum. Figure 2 Shown are the XRD patterns, surface morphology and energy spectrum of the prepared diamond.
[0045] Compared with Example 1, the extension of the plating time will significantly increase the thickness of the silicon carbide plated on the surface of the diamond particles.
[0046] Example 3
[0047] A method for coating a diamond surface with silicon carbide comprises the following steps:
[0048] S1. The diamond was ultrasonically cleaned for 30 min with a 10wt% hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral, and then the diamond was ultrasonically cleaned for 30 min in a 10wt% sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles;
[0049] S2. A silicon-gallium mixture having a silicon content of 1.5 wt% is placed in a crucible and heated to 1450°C in a non-oxygen environment. After being kept warm for 10 minutes, a silicon-gallium liquid phase medium with uniform silicon distribution is obtained; then, a diamond is placed in a heat-treated silicon-gallium liquid phase medium at a mass ratio of silicon to diamond of 1:20 and heated to 1200°C in a non-oxygen environment and kept warm for 10 minutes, and then cooled to form a coating on the surface of the diamond;
[0050] S3. Place the diamond with the coating on the surface in a centrifuge tube with a screen and centrifuge at 800r / min for 30min to remove the metal gallium attached to the diamond surface, dry, sieve, soak in 12wt% sodium hydroxide solution for 12h to remove excess silicon, wash with deionized water until neutral, dry and sieve to obtain diamond with silicon carbide coating on the surface. The surface of the obtained diamond is grayish white. The surface structure is determined to be SiC by XRD and energy spectrum. Figure 3 Shown are the XRD patterns, surface morphology and energy spectrum of the prepared diamond.
[0051] Compared with Example 1, the change in silicon content will affect the thickness of silicon carbide coated on the surface of diamond particles.
[0052] Example 4
[0053] A method for coating a diamond surface with silicon carbide comprises the following steps:
[0054] S1. The diamond was ultrasonically cleaned for 30 min with a 10wt% hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral, and then the diamond was ultrasonically cleaned for 30 min in a 10wt% sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles;
[0055] S2. A silicon-gallium mixture having a silicon content of 1.5 wt% is placed in a crucible and heated to 1450°C in a non-oxygen environment. After being kept warm for 10 minutes, a silicon-gallium liquid phase medium having uniform silicon distribution is obtained; then, a diamond is placed in a heat-treated silicon-gallium liquid phase medium at a mass ratio of silicon to diamond of 1:20 and heated to 1300°C in a non-oxygen environment and kept warm for 30 minutes, and then cooled to form a coating on the surface of the diamond;
[0056] S3. Place the diamond with the coating on the surface in a centrifuge tube with a screen and centrifuge at 800r / min for 30min to remove the metal gallium attached to the diamond surface, dry, sieve, soak in 12wt% sodium hydroxide solution for 12h to remove excess silicon, wash with deionized water until neutral, dry and sieve to obtain diamond with silicon carbide coating on the surface. The surface of the obtained diamond is grayish white. The surface structure is determined to be SiC by XRD and energy spectrum. Figure 4 Shown are the XRD patterns, surface morphology and energy spectrum of the prepared diamond.
[0057] Compared with Example 1, in addition to the plating time and silicon content, the increase in plating temperature also increases the thickness of silicon carbide on the surface of the diamond particles.
[0058] Example 5
[0059] A method for coating a diamond surface with silicon carbide comprises the following steps:
[0060] S1. The diamond was ultrasonically cleaned for 30 min with a 10wt% hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral, and then the diamond was ultrasonically cleaned for 30 min in a 10wt% sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles;
[0061] S2. A silicon-gallium mixture having a silicon content of 3 wt% is placed in a crucible and heated to 1450°C in a non-oxygen environment. After being kept warm for 10 minutes, a silicon-gallium liquid phase medium with uniform silicon distribution is obtained; then, a diamond is placed in a heat-treated silicon-gallium liquid phase medium at a mass ratio of silicon to diamond of 1:10 and heated to 1300°C in a non-oxygen environment and kept warm for 30 minutes, and then cooled to form a coating on the surface of the diamond;
[0062] S3. Place the diamond with the coating on the surface in a centrifuge tube with a screen and centrifuge at 800r / min for 30min to remove the metal gallium attached to the diamond surface, dry, sieve, soak in 12wt% sodium hydroxide solution for 12h to remove excess silicon, wash with deionized water until neutral, dry and sieve to obtain diamond with silicon carbide coating on the surface. The surface of the obtained diamond is grayish white. The surface structure is determined to be SiC by XRD and energy spectrum. Figure 5Shown are the XRD patterns, surface morphology and energy spectrum of the prepared diamond.
[0063] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for coating a diamond surface with silicon carbide, characterized in that: The steps include: S1. Sequentially wash the diamond with hydrochloric acid solution and sodium hydroxide solution to obtain pretreated diamond particles; S2. heat-treating the silicon-gallium mixture in a non-oxygen environment to obtain a silicon-gallium liquid phase medium, then mixing the pre-treated diamond particles obtained in step S1 with the silicon-gallium liquid phase medium, heating and maintaining the temperature in a non-oxygen environment to perform a plating reaction, and forming a coating on the diamond surface; S3. Place the coated diamond obtained in step S2 in a centrifuge tube with a screen and centrifuge, dry and sieve, soak with sodium hydroxide solution, wash with deionized water, dry and sieve to obtain diamond with silicon carbide coated on the surface.
2. The method according to claim 1, characterized in that In step S1, the diamond is ultrasonically cleaned with hydrochloric acid solution to remove surface metal impurities, and then washed with deionized water until neutral; then the diamond is ultrasonically cleaned with sodium hydroxide solution to remove surface grease, and then washed with deionized water until neutral, and then washed with alcohol one to three times, and dried to obtain pretreated diamond particles.
3. The method according to claim 1, characterized in that In step S1, the concentration of the hydrochloric acid solution is 10-15 wt %, and the concentration of the sodium hydroxide solution is 5-15 wt %.
4. The method according to claim 1, characterized in that: In step S2, the process of heat treating the silicon gallium liquid phase medium is: the temperature is 1410-1450° C., and the insulation time is 5-15 minutes; the plating reaction conditions are: the temperature is 1200-1300° C., and the insulation time is 10-30 minutes.
5. The method according to claim 1, characterized in that In the step S2, the silicon content in the silicon-gallium liquid phase medium is 1-9 wt%.
6. The method according to claim 1, characterized in that In the step S2, the mass ratio of silicon to diamond particles in the silicon-gallium liquid phase medium is 1:(10-100).
7. The method according to claim 1, characterized in that In the step S2, in the silicon-gallium liquid phase medium, the particle size of silicon is 1-3 μm; and the average particle size of diamond particles is 100-400 μm.
8. The method according to claim 1, characterized in that In step S3, the centrifugal conditions are: a rotation speed of 500 to 1000 r / min and a time of 5 to 30 min.
9. The method according to claim 1, characterized in that: In step S3, the concentration of the sodium hydroxide solution is 5 to 15 wt %, and the soaking time is 6 to 15 h.
10. A diamond with surface coated with silicon carbide prepared by the method according to any one of claims 1 to 9.