In-situ self-generated Al2O3 reinforced high entropy alloy coating and preparation method thereof
By generating a high-entropy alloy coating of Al2O3 reinforced phase in situ on the surface of titanium alloy, the problem of insufficient hardness and high-temperature oxidation resistance of titanium alloy is solved, achieving significant hardness increase and improvement of high-temperature oxidation resistance.
Patent Information
- Application Number
- CN202310195372.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Titanium alloys have low hardness, poor wear resistance, and insufficient high-temperature oxidation resistance in complex service environments, which limits their application performance.
In-situ self-generated Al2O3 is used to enhance the high-entropy alloy coating. By adding TiO2 to the AlTiVCrNb high-entropy alloy, laser cladding technology is used to generate Al2O3 as a reinforcing phase to improve the hardness and high-temperature oxidation resistance of the coating.
The hardness and high-temperature oxidation resistance of the TC4 matrix are significantly improved. The coating structure is uniform and dense, the density is appropriately reduced, the microhardness is increased by about 2.44 times, and the high-temperature oxidation resistance is improved by about 69%.
Smart Images

Figure HDA0004106967450000011 
Figure HDA0004106967450000012 
Figure HDA0004106967450000021
Abstract
Description
Technical Field
[0001] The invention discloses an in-situ self-generated Al2O3 enhanced high entropy alloy coating and a preparation method thereof, and belongs to the field of laser cladding. Background Art
[0002] Titanium alloys have the advantages of low density, high strength, good corrosion resistance, and high specific strength, and are widely used in many fields such as aerospace, petrochemicals, and automobiles. However, as a titanium alloy with excellent comprehensive performance, TC4 also presents some unique deficiencies in surface properties, such as low hardness, poor wear resistance, and insufficient high-temperature oxidation resistance, which seriously restricts the performance of titanium alloys in complex service environments.
[0003] The design concept of traditional alloys is usually to use one or two elements as the main components, and to improve some of the alloy properties by adding a small amount of other elements. With the rapid development of the exploration of advanced materials, practical alloys such as aluminum alloys, magnesium alloys, titanium alloys, and titanium-aluminum alloys have been developed, and traditional alloys like these have certain element limitations. In recent years, high-entropy materials have attracted the attention of researchers for their excellent combination of high strength, reasonable ductility, high-temperature thermal stability, excellent hardness, and mechanical properties. The design concept of high-entropy alloys breaks the traditional alloy design concept. It is generally composed of five or more elements, and the content of each element is between 5% and 35% (atomic fraction). High-entropy alloys have high entropy effects in thermodynamics, hysteresis diffusion effects in kinetics, lattice distortion effects, and cocktail effects in performance, which make high-entropy alloys have excellent comprehensive properties.
[0004] Metal-based composite coatings have high strength and good wear resistance. When different types and contents of particle reinforcement phases are added to high-entropy alloys, some reinforcement phases will decompose under the action of high-energy heat sources and form different types of secondary reinforcement phases with other elements in the metal matrix, thereby improving the comprehensive performance of the coating. At present, reinforcement phase materials mainly include ceramic materials such as Al2O3, WC, SiC and TiN. Al2O3 has high strength, high elastic modulus, high chemical stability, low cost and usually acts as a medium protective oxide, which is beneficial to improving the high-temperature oxidation resistance of the alloy. Summary of the invention
[0005] The purpose of the present invention is to provide an in-situ self-generated Al2O3 enhanced high entropy alloy coating, the coating is prepared from the following raw materials, the raw materials include the following mass percentage ratio of alloy powder: Al: 9.5-16.5%, Ti: 4-18%, V: 15.5-19%, Cr: 16-19.5%, Nb: 29-34.5%, TiO2: 0.5-18%. The coating prepared by the present invention has uniform distribution of reinforcement phase, fine structure, high hardness, excellent high temperature oxidation resistance, and can further effectively improve the high temperature oxidation resistance of TC4 substrate.
[0006] As a further optimization scheme of the present invention, the particle size range of the high entropy alloy powders Al, Ti, V, Cr, and Nb is 10 to 52 μm, and the particle size range of the TiO2 metal powder is 100 to 200 nm.
[0007] Another object of the present invention is to provide a method for preparing the in-situ self-generated Al2O3 enhanced high entropy alloy coating. Adding TiO2 to AlTiVCrNb can not only improve the laser absorption coefficient, but also combine the aluminothermic reaction with the laser cladding technology to promote the melting of the alloy powder while generating Al2O3 as a reinforcing phase distributed in the AlTiVCrNb high entropy alloy coating, which is beneficial to improving the metallurgical bonding between the cladding layer and the substrate and enhancing the high temperature oxidation resistance of the coating. The method specifically comprises the following steps:
[0008] (1) Surface pretreatment of the substrate.
[0009] (2) AlTiVCrNb-TiO2 high entropy alloy powder is weighed according to the proportion, and after weighing, a vacuum ball mill is used to mechanically mix the powder to obtain AlTiVCrNb-TiO2 high entropy alloy powder.
[0010] (3) The ball-milled powder was pre-deposited on the surface of the TC4 substrate to form a pre-deposited layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad, and a laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb-TiO2 high-entropy alloy coating.
[0011] Preferably, the pretreatment of the present invention is: grinding with 200 mesh, 400 mesh, 600 mesh sandpaper, cleaning, drying and standby.
[0012] Preferably, the parameters of the vacuum ball mill in step (2) of the present invention are: rotation speed 120 rpm, ball-to-material ratio 4:1, and ball milling time 1 h.
[0013] Preferably, the laser power of the laser cladding of the present invention is 1800W, the scanning speed is 600mm / min, the spot diameter is 4mm, the protective gas is helium, and the gas flow rate is 10L / min.
[0014] Principle of the present invention: The design of entropy alloy is mainly based on five major characteristics of high entropy alloy: high entropy effect in thermodynamics; slow diffusion effect in kinetics; lattice distortion effect in structure; "cocktail" effect in performance and high stability in organization, which make it have a variety of excellent properties, such as high hardness, extremely high high temperature strength, corrosion resistance, etc.; AlTiVCrNb is a high entropy alloy with a body-centered cubic (BCC) structure, which has excellent mechanical toughness, high hardness, high temperature oxidation resistance and corrosion resistance, etc., and the atomic bonding of the oxide ceramic phase is mainly ionic bonding, so most oxides have high melting point, good electrical insulation performance, high chemical stability and oxidation resistance. It is used as a basis to introduce Al2O3 as a strengthening phase for bonding, and a coating material with excellent comprehensive performance can be prepared, so as to improve the surface hardness and high temperature oxidation resistance of the TC4 substrate.
[0015] In the AlTiVCrNb system, TiO2 is added to prepare AlTiVCrNb-TiO2 high entropy alloy coating. Since the Gibbs free energy change of the reaction between Al and TiO2 is the most negative, that is, in the in-situ reaction process, Al and TiO2 are preferentially reacted to generate Al2O3 reinforcing phase distributed in the coating, thereby enhancing the comprehensive performance of the coating. By comparison, the performance of AlTiVCrNb-TiO2 high entropy alloy coating is significantly better than that of AlTiVCrNb coating without added TiO2.
[0016] The beneficial effects of the present invention are as follows:
[0017] (1) The AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding of the present invention has good metallurgical bonding with the substrate, and the cladding layer has a uniform and dense structure.
[0018] (2) The AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding of the present invention comprises light elements, which can enhance the coating performance and appropriately reduce the coating density.
[0019] (3) The AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding of the present invention, during the laser cladding process, the high energy input of the laser combined with the thermite reaction makes the inside of the molten pool instantly have a higher temperature and a faster cooling rate, resulting in the refinement of the internal grain structure of the coating, which plays a role in fine grain strengthening. Combined with the strengthening effect of the second phase Al2O3 generated by the in-situ reaction, the hardness of the TC4 substrate and the high-temperature oxidation resistance are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a macroscopic morphology of the coating prepared in Example 1;
[0021] Figure 2The microstructure of the coating prepared in Example 1;
[0022] Figure 3 It is a comparison chart of the oxidation kinetic curves of the coatings prepared in Examples 1, 2, 3 and Comparative Example 1. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the invention is not limited to the contents described above:
[0024] Example 1
[0025] The laser cladding powder composition of this embodiment is as follows: Al: 13.13%, Ti: 11.20%, V: 17.43%, Cr: 17.79%, Nb: 31.80%, TiO2: 8.65%; the TiO2 particle size range is: 100-200nm, and the particle size range of the remaining powders is 10-52μm; an electronic scale is used to weigh the powder of each element.
[0026] The method for preparing the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding in this embodiment comprises the following steps:
[0027] (1) The surface of the TC4 substrate is polished with 200 mesh, 400 mesh, and 600 mesh sandpaper, cleaned, and dried for later use.
[0028] (2) Weighing the metal powders according to the proportions and mixing them evenly by vacuum ball milling, wherein the vacuum ball milling speed is 120 rpm, the ball-to-powder ratio is 4:1, and the ball milling time is 1 h.
[0029] (3) The ball-milled powder was pre-placed on the surface of the TC4 substrate to form a pre-layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad. A laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb-TiO2 high-entropy alloy coating. The experimental parameters were as follows: laser power of 1800 W, scanning speed of 600 mm / min, spot diameter of 4 mm, protective gas of helium, and a gas flow rate of 10 L / min.
[0030] In this embodiment, the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding is cut into 6mmm×15mm×4mm blocks by a wire cutting machine, assisted by hydrogen peroxide resin for mounting, and ground and polished with 400 mesh, 600 mesh, 800 mesh, and 1200 mesh sandpaper to the metallographic requirements, corroded with a mixed solution of HNO3:Hf:H2O=1:2:7 for 15s, and rinsed with anhydrous ethanol and dried.
[0031] Figure 2This is the XRD diagram of the AlTiVCrNb-TiO2 high entropy alloy coating. It can be seen that the phase structure of the sample is mainly BCC phase and Al2O3.
[0032] Figure 3 This is the SEM image of the TiVCrNb-TiO2 high entropy alloy coating. It can be seen that Al2O3 is precipitated in the cladding layer, which can improve the hardness of the cladding layer. The surface hardness of the sample cladding layer is tested with a HDX-1000 Vickers microhardness tester. Five values are measured between the top of the cladding layer and the substrate. The maximum and minimum values are removed and the average value is taken. The test results show that the hardness of the substrate TC4 titanium alloy is 337.6HV 0.1 The average hardness of the cladding layer is 822.6HV 0.1 , which is about 2.44 times the hardness of the substrate. The high-temperature oxidation resistance of the AlTiVCrNb-TiO2 high-entropy alloy coating was measured using a tubular resistance furnace. The test temperature was 800°C and the test time was 100h. The oxidation kinetic curve was obtained as shown in Figure 3 As shown in Figure 2, the oxidation weight gain of the AlTiVCrNb-TiO2 high entropy alloy coating is only 13.31 mg cm -2 , which is about 69% lower than that of TC4 matrix, significantly improving its high temperature oxidation resistance.
[0033] Table 1 The surface hardness of the cladding layer of Example 1 is shown in the following table
[0034] Serial number Hardness value 1 Hardness value 2 Hardness value 3 Hardness value 4 Hardness value 5 average value TC4 332 347 358 329 322 337.6 Cladding layer 813 824 831 817 828 822.6
[0035] Example 2
[0036] The laser cladding powder composition of this embodiment is as follows: Al: 16.48%, Ti: 4.32%, V: 15.96%, Cr: 16.30%, Nb: 29.12%, TiO2: 17.82%; the TiO2 particle size range is: 100-200nm, and the particle size range of the remaining powders is 10-52μm; an electronic scale is used to weigh the powder of each element.
[0037] The method for preparing the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding in this embodiment comprises the following steps:
[0038] (1) The surface of the TC4 substrate is polished with 200 mesh, 400 mesh, and 600 mesh sandpaper, cleaned, and dried for later use;
[0039] (2) Weighing the metal powders according to the proportions and mixing them evenly by vacuum ball milling, wherein the vacuum ball milling speed is 120 rpm, the ball-to-powder ratio is 4:1, and the ball milling time is 1 h.
[0040] (3) The ball-milled powder was pre-placed on the surface of the TC4 substrate to form a pre-layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad. A laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb-TiO2 high-entropy alloy coating. The experimental parameters were as follows: laser power of 1800 W, scanning speed of 600 mm / min, spot diameter of 4 mm, protective gas of helium, and a gas flow rate of 10 L / min.
[0041] In this embodiment, the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding is cut into 6mm×15mm×4mm blocks by a wire cutting machine, assisted by hydrogen peroxide resin for mounting, and ground and polished to the metallographic requirements with 400 mesh, 600 mesh, 800 mesh, and 1200 mesh sandpapers, and corroded for 15s with a mixed solution of HNO3:Hf:H2O=1:2:7, and rinsed and dried with anhydrous ethanol; the surface hardness of the sample cladding layer is tested with a HDX-1000 Vickers microhardness tester, and five values are measured between the top of the cladding layer and the substrate. The maximum and minimum values are removed and the average value is taken. The test results show that the hardness of the substrate TC4 titanium alloy is 341.8HV 0.1 The average hardness of the cladding layer is 616.8HV 0.1 , which is about 1.8 times the hardness of the substrate; and a tubular resistance furnace was used to measure the high-temperature oxidation resistance of the AlTiVCrNb-TiO2 high-entropy alloy coating. The test temperature was 800℃ and the test time was 100h. The oxidation kinetic curve was obtained as shown in Figure 3 As shown in Figure 2, the oxidation weight gain of the AlTiVCrNb-TiO2 high entropy alloy coating is only 23.56 mg cm -2 , which is about 48.34% lower than that of TC4 matrix, significantly improving its high temperature oxidation resistance.
[0042] Table 2 The surface hardness of the cladding layer of Example 2 is shown in the following table
[0043] Serial number Hardness value 1 Hardness value 2 Hardness value 3 Hardness value 4 Hardness value 5 average value TC4 343 337 368 339 322 341.8 Cladding layer 625 623 610 598 628 616.8
[0044] Example 3
[0045] The laser cladding powder composition of this embodiment is as follows: Al: 9.97%, Ti: 17.56%, V: 18.62%, Cr: 19.06%, Nb: 34.07%, TiO2: 0.72%; the TiO2 particle size range is: 100-200nm, and the particle size range of the remaining powders is 10-52μm; an electronic scale is used to weigh the powder of each element.
[0046] The method for preparing the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding in this embodiment comprises the following steps:
[0047] (1) The surface of the TC4 substrate is polished with 200 mesh, 400 mesh, and 600 mesh sandpaper, cleaned, and dried for later use.
[0048] (2) Weighing the metal powders according to the proportions and mixing them evenly by vacuum ball milling, wherein the vacuum ball milling speed is 120 rpm, the ball-to-powder ratio is 4:1, and the ball milling time is 1 h.
[0049] (3) The ball-milled powder was pre-placed on the surface of the TC4 substrate to form a pre-layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad. A laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb-TiO2 high-entropy alloy coating. The experimental parameters were as follows: laser power of 1800 W, scanning speed of 600 mm / min, spot diameter of 4 mm, protective gas of helium, and a gas flow rate of 10 L / min.
[0050] In this embodiment, the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding is cut into 6mm×15mm×4mm blocks by a wire cutting machine, assisted by hydrogen peroxide resin for mounting, and ground and polished to metallographic requirements with 400 mesh, 600 mesh, 800 mesh, and 1200 mesh sandpapers, and corroded for 15s with a mixed solution of HNO3:Hf:H2O=1:2:7, and rinsed and dried with anhydrous ethanol. The surface hardness of the sample cladding layer is tested with a HDX-1000 Vickers microhardness tester, and five values are measured between the top of the cladding layer and the substrate. The average value is taken after removing the maximum and minimum values. The test results show that the hardness of the substrate TC4 titanium alloy is 345.4HV 0.1 The average hardness of the cladding layer is 584.0HV 0.1 , which is about 1.69 times the hardness of the substrate; and a tubular resistance furnace was used to measure the high-temperature oxidation resistance of the AlTiVCrNb-TiO2 high-entropy alloy coating. The test temperature was 800℃ and the test time was 100h. The oxidation kinetic curve was obtained as shown in Figure 3 As shown in Figure 2, the oxidation weight gain of the AlTiVCrNb-TiO2 high entropy alloy coating is only 29.83 mg cm -2 , which is about 34.08% lower than that of TC4 matrix, significantly improving its high temperature oxidation resistance.
[0051] Table 3 The surface hardness of the cladding layer of Example 3 is shown in the following table
[0052] Serial number Hardness value 1 Hardness value 2 Hardness value 3 Hardness value 4 Hardness value 5 average value TC4 346 352 346 352 331 345.4 Cladding layer 596 592 581 579 572 584.0
[0053] Comparative Example 1
[0054] The laser cladding powder of this embodiment has the following composition: Al: 9.90%, Ti: 17.68%, V: 18.82%, Cr: 19.21%, Nb: 34.32%; wherein the particle size range of the metal alloy powder is 10 to 52 μm; and each element powder is weighed using an electronic scale.
[0055] The method for preparing the AlTiVCrNb high entropy alloy coating obtained by laser cladding in this embodiment comprises the following steps:
[0056] (1) The surface of the TC4 substrate is polished with 200 mesh, 400 mesh, and 600 mesh sandpaper, cleaned, and dried for later use.
[0057] (2) Weighing the metal powders according to the proportions and mixing them evenly by vacuum ball milling, wherein the vacuum ball milling speed is 120 rpm, the ball-to-powder ratio is 4:1, and the ball milling time is 1 h.
[0058] (3) The ball-milled powder was pre-placed on the surface of the TC4 substrate to form a pre-layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad. A laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb high-entropy alloy coating. The experimental parameters were as follows: laser power of 1800 W, scanning speed of 600 mm / min, spot diameter of 4 mm, protective gas of helium, and a gas flow rate of 10 L / min.
[0059] In this embodiment, the AlTiVCrNb-TiO2 high entropy alloy coating obtained by laser cladding is cut into 6mm×15mm×4mm blocks by a wire cutting machine, assisted by hydrogen peroxide resin for mounting, and ground and polished to metallographic requirements with 400 mesh, 600 mesh, 800 mesh, and 1200 mesh sandpapers, and corroded for 15s with a mixed solution of HNO3:Hf:H2O=1:2:7, and rinsed and dried with anhydrous ethanol. The surface hardness of the sample cladding layer is tested with a HDX-1000 Vickers microhardness tester, and five values are measured between the top of the cladding layer and the substrate. The average value is taken after removing the maximum and minimum values. The test results show that the hardness of the substrate TC4 titanium alloy is 345.0HV 0.1 The average hardness of the cladding layer is 528.6HV0.1, which is about 1.53 times the hardness of the substrate. The high-temperature oxidation resistance of the AlTiVCrNb high-entropy alloy coating was measured using a tubular resistance furnace. The test temperature was 800℃ and the test time was 100h. The oxidation kinetic curve was obtained as shown in Figure 3 As shown in Figure 2, the oxidation weight gain of the AlTiVCrNb high entropy alloy coating is only 32.52 mg cm -2 , which is about 28.24% lower than that of TC4 matrix, improving its high temperature oxidation resistance.
[0060] Table 4 The surface hardness of the cladding layer of Example 4 is shown in the following table
[0061] Serial number Hardness value 1 Hardness value 2 Hardness value 3 Hardness value 4 Hardness value 5 average value TC4 346 353 341 345 340 345.0 Cladding layer 548 534 525 521 515 528.6
[0062] Comparing Example 1 with Examples 1, 2, and 3, it can be seen that the hardness of the AlTiVCrNb-TiO2 high entropy alloy coating with TiO2 added is significantly greater than that of the AlTiVCrNb high entropy alloy coating without TiO2 added. Figure 3 It can be clearly seen that the oxidation weight gain of the AlTiVCrNb-TiO2 high entropy alloy coating with the addition of TiO2 is significantly lower than that of the AlTiVCrNb high entropy alloy coating without the addition of TiO2, indicating that with the addition of TiO2 to the AlTiVCrNb high entropy alloy coating, the Al2O3 generated by the in-situ reaction acts as a reinforcing phase in the coating, which plays a promoting role and improves the hardness and high-temperature oxidation resistance of the coating.
[0063] In summary, the AlTiVCrNb-based high entropy alloy coatings all improve the hardness and high-temperature oxidation resistance of the TC4 substrate, and with the addition of TiO2 in the AlTiVCrNb-based high entropy alloy coatings, the hardness and high-temperature oxidation resistance of the coatings change. Among them, the AlTiVCrNb-TiO2 high entropy alloy coating with a TiO2 mass ratio of 8.65% has the best performance (Example 1), and its microhardness is as high as 822.6HV 0.1 , which is about 2.44 times the hardness of the substrate, and the coating oxidation weight gain is only 13.31 mg cm -2 , which is about 69% lower than that of TC4 substrate, significantly improving its high-temperature oxidation resistance. The mechanism of performance improvement is as follows: (1) Due to the rapid cooling and heating of laser cladding, the internal grains of the coating are refined, resulting in fine grain strengthening; (2) After adding TiO2 to the AlTiVCrNb high-entropy alloy coating, Al2O3 is generated in situ as a reinforcing phase distributed in the coating, playing a role of second phase strengthening; (3) Due to the unique solid solution strengthening effect of high-entropy alloys; ultimately, the hardness of the coating is improved and the high-temperature oxidation resistance is good.
[0064] The hardness and high temperature oxidation resistance of the AlTiVCrNb-TiO2 high entropy alloy coating with a TiO2 mass ratio of 17.82% are reduced. This is because with the addition of TiO2, the heat released by the in-situ reaction will increase, causing the Ti element inside the coating to be diluted into the coating, forming an α-Ti phase in the coating, thereby reducing the volume fraction of the BCC phase in the coating, resulting in a decrease in its hardness and high temperature oxidation resistance. Therefore, the present invention selects the best example as Example 1.
Claims
1. A method for preparing an in-situ self-generated Al2O3 enhanced high entropy alloy coating, characterized in that: The specific steps include: (1) Surface pretreatment of substrate: (2) weighing AlTiVCrNb-TiO2 high entropy alloy powder according to the proportion, and after weighing, using a vacuum ball mill to mechanically mix; (3) The ball-milled powder was pre-deposited on the surface of the TC4 substrate to form a pre-deposited layer. A fiber laser was used to place the laser head perpendicular to the surface to be clad. A laser cladding test was carried out under the protection of helium to prepare an AlTiVCrNb-TiO2 high-entropy alloy coating. The coating is prepared from the following raw materials, which include alloy powders in the following mass percentages: Al: 9.5-16.5%, Ti: 4-18%, V: 15.5-19%, Cr: 16-19.5%, Nb: 29-34.5%, TiO2: 8.65%; The particle size range of the high entropy alloy powders Al, Ti, V, Cr and Nb is 10-52 μm, and the particle size range of the TiO2 metal powder is 100-200 nm.
2. The method for preparing the in-situ self-generated Al2O3 enhanced high entropy alloy coating according to claim 1, characterized in that: The pretreatment is as follows: polish with 200 mesh, 400 mesh, and 600 mesh sandpaper, clean, and dry for use.
3. The method for preparing the in-situ self-generated Al2O3 enhanced high entropy alloy coating according to claim 1, characterized in that: The parameters of the vacuum ball mill in step (2) are: rotation speed 120 rpm, ball-to-material ratio 4:1, and ball milling time 1 h.
4. The method for preparing the in-situ self-generated Al2O3 enhanced high entropy alloy coating according to claim 1, characterized in that: The laser power of laser cladding is 1800W, the scanning speed is 600mm / min, the spot diameter is 4mm, the protective gas is helium, and its gas flow rate is 10L / min.