A low-carbon resource utilization shield inert synchronous grouting material and preparation method thereof
By comprehensively utilizing solid waste resources such as iron desulfurization slag, iron tailings and waste concrete, low-carbon resource utilization shield inert synchronous grouting materials are prepared, which solves the problems of large amount of natural sand and low mechanical properties, and achieves high efficiency of resources Utilization and stability requirements for tunnel engineering.
Patent Information
- Application Number
- CN202211651222.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-21
AI Technical Summary
The amount of natural sand in existing shield grouting materials is large, resulting in waste of resources and environmental damage. The construction properties of active grouting materials are poor, and the mechanical properties of inert grouting materials are low, making it difficult to replace the use of cement.
Using low-carbon resource utilization shield inert synchronous grouting materials, the materials with high mechanical properties and good construction properties are prepared by comprehensively utilizing solid waste resources such as iron desulfurization slag, iron tailings, and waste concrete to replace traditional natural sand and cement.
It realizes efficient utilization of resources, reduces energy consumption and costs, and the materials have the characteristics of high early strength and good construction properties. They can effectively replace traditional grouting materials and meet the stability needs of tunnel projects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of comprehensive utilization of solid waste resources, and specifically relates to a low-carbon resource utilization type shield inert synchronous grouting material and a preparation method thereof. Background Art
[0002] The shield method is a construction method commonly used in tunnel engineering. During the shield method construction, there will be a shield tail gap of about 5 to 15 cm between the prefabricated segments released from the shield tail and the soil. This gap needs to be poured and grouted synchronously to avoid soil settlement, segment water seepage and other problems, and maintain the stability of the entire tunnel structure. Shield grouting materials are divided into active grouting materials and inert grouting materials according to whether they contain cement. Comparing the two, active grouting materials have relatively high mechanical performance indicators and strong site adaptability, but relatively poor construction performance and are easy to block pipes; inert grouting materials have good construction performance and are not easy to block pipes, but their mechanical performance indicators are relatively low. In actual engineering, both active grouting materials and inert grouting materials are used. Relatively speaking, the former has better mechanical properties and is therefore more widely used. However, the production of cement has high energy consumption characteristics and high consumption of primary resources. Therefore, reducing its use and replacing it with alternatives has become the goal of the industry to develop shield inert grouting materials that can overcome resource waste and have good mechanical properties.
[0003] In addition, sand is the main admixture in both active and inert grouting materials, and the amount used is large. The amount of natural sand and other construction materials that consume primary resources used in grouting materials has increased dramatically, resulting in a continuous increase in prices and serious damage to the ecological environment. Finding technical methods that can replace natural sand is also an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to provide a low-carbon resource utilization type shield inert synchronous grouting material, which comprehensively utilizes molten iron desulfurization slag, iron tailings and waste concrete, has high solid waste resource utilization rate, good mechanical properties and good construction performance.
[0005] The present invention adopts the following technical scheme: a low-carbon resource utilization type shield inert synchronous grouting material, comprising the following raw materials in weight percentage: 13% to 20% of inert cementitious material, 15.2% to 19.5% of water, 15% to 20% of iron tailings sand, 25% to 31% of river sand, 3% to 4% of waste concrete, 5% to 6% of sodium bentonite, 6% to 7% of ultrafine powder of molten iron desulfurization slag, 3% to 4% of alkali activator, 0.2% to 0.5% of water reducer, and 1.5% to 2.5% of admixture, and the total content of the above raw materials is 100%.
[0006] Furthermore, the inert cementitious material is a mixture of slag powder, metakaolin and silica fume, wherein the mass ratio of slag powder, metakaolin and silica fume is (8-11): (3-5): (2-4).
[0007] Furthermore, the effective components of the ultrafine powder of molten iron desulfurization slag are SO3, CaO, SiO2 and Al2O3, wherein the mass content of SO3 is 1.5%~2.5%, and the particle size grade of the ultrafine powder of molten iron desulfurization slag is 800 mesh.
[0008] Furthermore, the particle size of the river sand is 0.2 mm to 0.5 mm, the particle size of the iron tailings sand is 0.2 mm to 0.5 mm, and the particle size of the waste concrete is 0.2 mm to 0.5 mm.
[0009] Furthermore, the additive is a silane coupling agent composite solution, and the silane coupling agent composite solution is composed of the following components in percentage by mass: 25% silane coupling agent, 70% acetone and 5% water.
[0010] Furthermore, the water reducing agent is a powdered polycarboxylic acid high-efficiency water reducing agent.
[0011] The present invention also discloses a method for preparing the above-mentioned low-carbon resource utilization type shield inert synchronous grouting material, and the preparation method is as follows:
[0012] Step 1: Under the condition of 130° C. to 150° C., slag powder, metakaolin and iron tailings sand are separately mixed with the composite solution of the admixture silane coupling agent by magnetic stirring to obtain modified slag powder, modified metakaolin and modified iron tailings sand respectively;
[0013] Step 2: Mixing the modified slag powder, modified metakaolin and silica fume at room temperature, and stirring with a constant temperature magnetic force to obtain an inert gelling material;
[0014] Step 3: mixing inert cementitious material powder, modified iron tailings sand, river sand, waste concrete, sodium bentonite, ultrafine iron molten desulfurization slag powder, and powdered polycarboxylic acid high-efficiency water reducing agent at room temperature to obtain a powder mixture;
[0015] Step 4: Mixing the alkaline activator with water at room temperature, and stirring with a constant temperature magnetic force to obtain an alkaline activator solution;
[0016] Step 5: Mix the powder mixture in step 3 with the alkaline activator solution in step 4, and stir them with a constant temperature magnetic force to obtain a low-carbon resource utilization shield inert synchronous grouting material.
[0017] The beneficial effects of the present invention are as follows: 1. Solid waste resources are used as the main raw materials, and the solid waste material reaches 20%. There is no cement, which reduces energy consumption and saves costs. The prepared low-carbon resource utilization shield inert synchronous grouting material has the characteristics of good mechanical properties, high early strength and good construction performance. 2. The hot metal desulfurization slag contains relatively high f-CaO and f-MgO, which can react with the silicon and aluminum components in the iron tailings and waste concrete as geopolymers through alkali excitation to generate geopolymerization reactions. The generated geopolymer gel can effectively fill the pores of the material, increase the density of the material, and improve the mechanical properties of the material. 3. The iron tailings and waste concrete themselves can be used as fine aggregates to replace natural sand. 4. Silica fume, metakaolin, slag powder, and iron tailings sand are all inorganic materials, and they have good compatibility. Therefore, silica fume can be combined with metakaolin, slag powder, and iron tailings sand to form an inert cementitious material, and silica fume can be dispersed into the structure of the inert cementitious material to form a dense structure bond with good interface compatibility. DETAILED DESCRIPTION
[0018] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0019] The invention discloses a low-carbon resource utilization type shield inert synchronous grouting material. The synchronous grouting material comprises the following raw materials in percentage by weight: 13%-20% of inert cementitious material, 15.2%-19.5% of water, 15%-20% of iron tailings sand, 25%-31% of river sand, 3%-4% of waste concrete, 5%-6% of sodium bentonite, 6%-7% of ultrafine powder of molten iron desulfurization slag, 3%-4% of alkali activator, 0.2%-0.5% of water reducer, and 1.5%-2.5% of admixture, and the total content of the above raw materials is 100%.
[0020] Among them: the inert cementitious material is a mixture of slag powder, metakaolin and silica fume, wherein the mass ratio of slag powder, metakaolin and silica fume is (8~11): (3~5): (2~4).
[0021] The above-mentioned slag powder is S95 grade granulated blast furnace slag powder, the specific surface area of the slag powder is 370~400, and the particle size grade is 400 mesh. The above-mentioned metakaolin activity index is ≥110, and the particle size grade is 1250 mesh. The above-mentioned silica fume has a specific surface area of 23700 and a particle size grade of 10000 mesh.
[0022] The fineness of silica fume is 10000 mesh, with the characteristics of large specific surface area and good dispersibility. Silica fume, metakaolin, slag powder and iron tailings are all inorganic materials with good compatibility. Therefore, silica fume can be combined with metakaolin, slag powder and iron tailings to form an inert cementitious material, and silica fume can be dispersed into the structure of the inert cementitious material to form a dense structure bond with good interface compatibility.
[0023] Due to its high content of aluminate, kaolin can form silicate gel with Ca in slag powder, Si and Al in iron tailings, and Si in silica fume in an alkaline excitation environment, and then form aluminosilicate early strength gel. This can improve the overall mechanical properties of the inert cementitious material and provide good early strength.
[0024] The particle size of the above iron tailings is in the range of 0.2mm~0.5mm. On the one hand, the particle size of the iron tailings is 0.2mm~0.5mm, and it has a high silicon dioxide content. Its particle size and properties are similar to those of medium sand and can replace sand as fine aggregate. On the other hand, under the action of the alkaline environment, the quartz body of inactive silicon contained in the iron tailings is stimulated to produce a certain amount of gel, filling the gaps in the inert gelling material and improving the mechanical properties.
[0025] The particle sizes of the above river sands are all in the range of 0.2mm~0.5mm.
[0026] The particle size of the above waste concrete sand is in the range of 0.2mm~0.5mm. The waste concrete particles have aggregate effect, and the aggregate contains, which can produce -Si-O-Al-O-based aluminosilicate geopolymer gel with a spatial network structure through geopolymerization reaction with alkali activator, which coexists in the matrix with the silicate system produced by alkali activation of inert gelling material, and synergistically promotes the strength development of the material.
[0027] The effective components of the hot metal desulfurization slag ultrafine powder are SO3, CaO, SiO2 and Al2O3, among which the SO3 content is 1.5%~2.5% and the particle size grade is 800 mesh. Hot metal desulfurization slag ultrafine powder has the properties of mineral powder after grinding due to the special process different from steel slag production; at the same time, hot metal desulfurization slag ultrafine powder contains a certain amount of sulfate, so an appropriate amount of hot metal desulfurization slag ultrafine powder can form a sulphoaluminate gelling system with metakaolin and silica fume to improve the early strength of the grouting material; at the same time, the f-CaO and f-MgO in the hot metal desulfurization slag ultrafine powder can undergo hydration reaction to form a micro-expanded crystalline hydrate calcium sulfonate, which can compensate for the shrinkage of the material and improve the density of the material within a certain range.
[0028] The alkaline activator is sodium silicate, and the sodium silicate is sodium silicate nonahydrate;
[0029] The admixture is a silane coupling agent composite solution, which includes the following components in mass percentage: 25% silane coupling agent, 70% acetone, and 5% water, wherein the silane coupling agent is KH-560. The water reducer is a powdered polycarboxylic acid high-efficiency water reducer.
[0030] The silane coupling agent in the silane coupling agent composite solution has a silane alkoxy group. Under the action of the dispersant acetone, the above functional groups are uniformly attached to the surface of inorganic materials such as metakaolin, slag powder, and iron tailings sand. On the one hand, it is beneficial to improve the dispersibility of the material, increase the specific surface area of the hydration reaction of the modified inorganic material, and the interaction area between silica fume and the modified inorganic material, and improve the workability and mechanical properties of the inert gelling material. On the other hand, it can improve the surface properties of the material, promote the surface of the modified inorganic material to have hydrophobicity, and is beneficial to reduce the water film thickness between particles during the hydration process of silica fume and the modified inorganic material, improve the density of the hydrated agglomerate, and reduce the porosity of the inert gelling material to improve its density.
[0031] The preparation method of the low-carbon resource utilization shield inert synchronous grouting material is as follows:
[0032] Step 1: Using a high-temperature magnetic stirrer at 130°C to 150°C, slag powder, metakaolin, and iron tailings are separately mixed with the composite solution of the silane coupling agent admixture, with a stirring speed of 150r / min to 180r / min and a stirring time of 15min to 30min to obtain modified slag powder, modified metakaolin, and modified iron tailings.
[0033] Step 2: Use a constant temperature magnetic stirrer to mix the modified slag powder, modified metakaolin and silica fume at room temperature at a stirring speed of 150 r / min to 180 r / min and a stirring time of 10 min to 30 min to obtain an inert cementitious material powder.
[0034] Step 3: Use a constant temperature magnetic stirrer to mix the inert cementitious material powder, modified iron tailings sand, river sand, waste concrete, sodium bentonite, molten iron desulfurization slag ultrafine powder, and powdered polycarboxylic acid high-efficiency water reducer at room temperature with a stirring speed of 150 r / min~180 r / min and a stirring time of 10 min~20 min to obtain a powder mixture.
[0035] Step 4: Use a constant temperature magnetic stirrer to mix the alkaline activator and water at room temperature, with a stirring speed of 150 r / min~180 r / min and a stirring time of 20 min~30 min to obtain an alkaline activator solution.
[0036] Step 5: Use a constant temperature magnetic stirrer to mix the powder mixture prepared in step 3 with the alkali-activated solution prepared in step 4 at room temperature, with a stirring speed of 150 r / min~180 r / min and a stirring time of 10 min~25 min to obtain a low-carbon resource utilization shield inert synchronous grouting material.
[0037] In the method for preparing a low-carbon resource utilization type shield inert synchronous grouting material of the present invention, room temperature refers to the temperature of the test site, that is, no additional heating is required.
[0038] Example 1
[0039] Taking the preparation of 100g of a low-carbon resource utilization shield inert synchronous grouting material as an example, the components used and their mass ratios are: 8% slag powder, 3% kaolin, 2% silica fume, 15% iron tailings sand, 31% river sand, 4% waste concrete, 5.2% sodium bentonite, 7% ultrafine iron molten desulfurization slag powder, 19.5% water, 3% alkali activator, 0.3% water reducer, and 2% admixture.
[0040] The mesh number of slag powder is 400 mesh, and the specific surface area is 380. The mesh number of metakaolin is 1250 mesh, and the activity index is ≥110. The silica fume is 10000 mesh, and the specific surface area is 23700. The particle size of river sand is in the range of 0.2mm~0.5mm. The effective components of hot metal desulfurization slag ultrafine powder are SO3, CaO, SiO2 and Al2O3, among which the SO3 content is about 2.2%, and the particle size grade of hot metal desulfurization slag ultrafine powder is 800 mesh.
[0041] The admixture is a silane coupling agent composite solution, which is composed of the following components in mass percentage: 25% silane coupling agent, 70% acetone and 5% water, and the silane coupling agent is KH-560. The alkali activator is sodium silicate. The water reducer is a powdered polycarboxylic acid high-efficiency water reducer.
[0042] The preparation method of the low-carbon resource utilization shield inert synchronous grouting material is as follows:
[0043] Step 1: Use a high-temperature magnetic stirrer to mix the slag powder, kaolin and the composite solution of the silane coupling agent admixture at 140° C., with a stirring speed of 150 r / min and a stirring time of 15 min to obtain modified slag powder and modified kaolin.
[0044] Step 2: Use a constant temperature magnetic stirrer to mix the modified slag powder, modified metakaolin and silica fume at room temperature at a stirring speed of 160 r / min and a stirring time of 25 min to obtain an inert cementitious material powder.
[0045] Step 3: Use a constant temperature magnetic stirrer to mix the inert cementitious material powder, river sand, waste concrete, sodium bentonite, molten iron desulfurization slag ultrafine powder, and powdered polycarboxylic acid high-efficiency water reducing agent at room temperature with a stirring speed of 180 r / min and a stirring time of 15 min to obtain a powder mixture.
[0046] Step 4: Use a constant temperature magnetic stirrer to mix the alkaline activator and water at room temperature, with a stirring speed of 160 r / min and a stirring time of 25 min to obtain an alkaline activator solution.
[0047] Step 5: Use a constant temperature magnetic stirrer to mix the powder mixture prepared in step 3 with the alkaline activator solution prepared in step 4 at room temperature, with a stirring speed of 180 r / min and a stirring time of 25 min to obtain a low-carbon resource utilization shield inert synchronous grouting material.
[0048] Example 2
[0049] The differences between this embodiment and Embodiment 1 are listed below, and the contents not listed are the same.
[0050] Taking the preparation of 100g of a low-carbon resource utilization shield inert synchronous grouting material as an example, the components used and their mass ratios are: slag powder 11%, kaolin 3%, silica fume 2%, iron tailings sand 20%, river sand 29%, waste concrete 3%, sodium bentonite 5.5%, molten iron desulfurization slag ultrafine powder 6%, water 15.3%, alkali activator 3.3%, water reducer 0.4%, and admixture 1.5%.
[0051] The preparation method of a low-carbon resource utilization shield inert synchronous grouting material in this embodiment is the same as the preparation method of implementation 1, the difference is the reaction conditions in each step, the different reaction conditions are now listed, and the parts not listed are the same content.
[0052] In step 1, a high temperature magnetic stirrer is used at 130° C. for 20 min.
[0053] In step 2, the stirring speed is 180 r / min.
[0054] In step three, the stirring speed is 150 r / min and the stirring time is 15 min to obtain a powder mixture.
[0055] In step 4, the stirring speed is 150 r / min and the stirring time is 20 min.
[0056] In step 5, the stirring speed is 180 r / min and the stirring time is 10 min.
[0057] Example 3
[0058] The differences between this embodiment and embodiment 1 are listed below, and the contents not listed are the same. Taking the preparation of 100g of low-carbon resource utilization shield inert synchronous grouting material as an example, the components used and their mass ratios are: 10% slag powder, 5% metakaolin, 3% silica fume, 16% iron tailings sand, 27% river sand, 4% waste concrete, 5% sodium bentonite, 6.2% ultrafine powder of hot metal desulfurization slag, 17.1% water, 4% alkali activator, 0.2% water reducer, and 2.5% admixture.
[0059] The preparation method of a low-carbon resource utilization shield inert synchronous grouting material in this embodiment is the same as the preparation method of implementation 1, the difference is the reaction conditions in each step, the different reaction conditions are now listed, and the parts not listed are the same content.
[0060] In step 1, a high temperature magnetic stirrer is used at 150° C., with a stirring speed of 150 r / min and a stirring time of 25 min.
[0061] In step 2, the stirring speed is 180 r / min and the stirring time is 20 min.
[0062] In step three, the stirring speed is 150 r / min and the stirring time is 20 min to obtain a powder mixture.
[0063] In step 4, the stirring speed is 160 r / min and the stirring time is 30 min.
[0064] In step 5, the stirring speed is 170 r / min and the stirring time is 25 min.
[0065] Example 4
[0066] The differences between this embodiment and Embodiment 1 are listed below, and the contents not listed are the same.
[0067] Taking the preparation of 100g of low-carbon resource utilization shield inert synchronous grouting material as an example, the components used and their mass ratios are: slag powder 10.6%, kaolin 4.7%, silica fume 7%, iron tailings sand 18%, river sand 25%, waste concrete 3%, sodium bentonite 6%, molten iron desulfurization slag ultrafine powder 6.5%, water 15.2%, alkali activator 3.8%, water reducer 0.5%, and admixture 2%.
[0068] The preparation method of a low-carbon resource utilization shield inert synchronous grouting material in this embodiment is the same as the preparation method of implementation 1, the difference is the reaction conditions in each step, the different reaction conditions are now listed, and the parts not listed are the same content.
[0069] In step 1, a high temperature magnetic stirrer is used at 140° C., with a stirring speed of 180 r / min and a stirring time of 20 min.
[0070] In step 2, the stirring speed is 170 r / min and the stirring time is 25 min.
[0071] In step three, the stirring speed is 150 r / min and the stirring time is 20 min to obtain a powder mixture.
[0072] In step 4, the stirring speed is 180 r / min and the stirring time is 25 min.
[0073] In step 5, the stirring speed is 150 r / min and the stirring time is 20 min.
[0074] Comparative Example 1
[0075] A shield inert synchronous grouting material, taking the preparation of 100g product as an example, the components used and their mass ratio are: 10% slag powder, 5% metakaolin, 3% silica fume, 47% river sand, 5% sodium bentonite, 6.2% ultrafine iron molten desulfurization slag powder, 17.1% water, 4% alkali activator, 0.2% water reducer, and 2.5% admixture.
[0076] The mesh number of slag powder is 400 mesh, and the specific surface area is 380. The mesh number of metakaolin is 1250 mesh, and the activity index is ≥110. The silica fume is 10000 mesh, and the specific surface area is 23700. The particle size of river sand is in the range of 0.2mm~0.5mm.
[0077] The effective components of the ultrafine powder of molten iron desulfurization slag are SO3, CaO, SiO2 and Al2O3, among which the SO3 content is about 2.2%, and the particle size grade of the ultrafine powder of molten iron desulfurization slag is 800 mesh.
[0078] The admixture is a silane coupling agent composite solution, which includes the following components in mass percentage: 25% silane coupling agent, 70% acetone, and 5% water, wherein the silane coupling agent is KH-560. The alkali activator is sodium silicate. The water reducer is a powdered polycarboxylic acid high-efficiency water reducer.
[0079] Comparative Example 2
[0080] A shield inert synchronous grouting material, taking the preparation of 100g of the product as an example, the components used and their mass ratios are: 10% slag powder, 5% metakaolin, 3% silica fume, 16% iron tailings sand, 27% river sand, 4% waste concrete, 5% sodium bentonite, 6.2% ultrafine powder of molten iron desulfurization slag, 19.6% water, 4% alkali activator, and 0.2% water reducer.
[0081] The mesh number of slag powder is 400 mesh, and the specific surface area is 380. The mesh number of metakaolin is 1250 mesh, and the activity index is ≥110. The mesh number of silica fume is 10000 mesh, and the specific surface area is 23700.
[0082] The particle size of iron ore tailings is in the range of 0.2mm~0.5mm. The particle size of river sand is in the range of 0.2mm~0.5mm. The particle size of waste concrete is in the range of 0.2mm~0.5mm.
[0083] The effective components of the above-mentioned ultrafine powder of molten iron desulfurization slag are SO3, CaO, SiO2 and Al2O3, among which the SO3 content is about 2.2%, and the particle size grade of the ultrafine powder of molten iron desulfurization slag is 800 mesh.
[0084] The alkali activator is sodium silicate, and the water reducer is powdered polycarboxylic acid high-efficiency water reducer.
[0085] The preparation method of the above-mentioned shield inert synchronous grouting material is as follows:
[0086] 1. Using a constant temperature magnetic stirrer, slag powder, silica fume and metakaolin are mixed at room temperature at a stirring speed of 160 r / min and a stirring time of 25 min to obtain an inert cementitious material powder.
[0087] 2. Using a constant temperature magnetic stirrer, inert cementitious material powder, iron tailings sand, river sand, waste concrete, sodium bentonite, molten iron desulfurization slag ultrafine powder, and powdered polycarboxylic acid high-efficiency water reducing agent are mixed at room temperature at a stirring speed of 180r / min and a stirring time of 15min to obtain a powder mixture.
[0088] 3. Using a constant temperature magnetic stirrer at room temperature, the base activator and water were mixed at a stirring speed of 160 r / min and a stirring time of 25 min to obtain a base activator solution.
[0089] 4. The powder mixture was mixed with the alkaline activator solution at room temperature using a constant temperature magnetic stirrer at a stirring speed of 180 r / min and a stirring time of 25 min to obtain a low-carbon resource utilization shield inert synchronous grouting material.
[0090] Comparative Example 3
[0091] A shield inert synchronous grouting material, taking the preparation of 100g product as an example, the components used and their mass ratios are: 18% silicate cement, 16% iron tailings sand, 27% river sand, 4% waste concrete, 5% sodium bentonite, 6.2% ultrafine powder of molten iron desulfurization slag, 17.1% water, 4% alkali activator, 0.2% water reducer, and 2.5% admixture.
[0092] The particle sizes of the iron tailings are all within the range of 0.2 mm to 0.5 mm. The particle sizes of the river sand are all within the range of 0.2 mm to 0.5 mm. The particle sizes of the waste concrete are all within the range of 0.2 mm to 0.5 mm. The silicate cement is Conch PO42.5, which is produced by Conch Cement.
[0093] The effective components of the ultrafine powder of molten iron desulfurization slag are SO3, CaO, SiO2 and Al2O3, among which the SO3 content is about 2.2%, and the particle size grade of the ultrafine powder of molten iron desulfurization slag is 800 mesh.
[0094] The admixture is a silane coupling agent composite solution, which includes the following components in mass percentage: 25% silane coupling agent, 70% acetone, and 5% water, wherein the silane coupling agent is KH-560. The alkali activator is sodium silicate, and the water reducer is a powdered polycarboxylic acid high-efficiency water reducer.
[0095] The preparation method of the above-mentioned shield inert synchronous grouting material is as follows:
[0096] 1. Using a high temperature magnetic stirrer, the iron tailings and the composite solution of the silane coupling agent additive were mixed at 140° C. The stirring speed was 150 r / min and the stirring time was 15 min to obtain modified iron tailings.
[0097] 2. Using a constant temperature magnetic stirrer, the modified iron tailings sand, river sand, waste concrete, sodium bentonite, silicate cement, and powdered polycarboxylic acid high-efficiency water reducing agent were mixed at room temperature at a stirring speed of 180 r / min and a stirring time of 15 min to obtain a powder mixture.
[0098] 3. Using a constant temperature magnetic stirrer at room temperature, the base activator and water were mixed at a stirring speed of 160 r / min and a stirring time of 25 min to obtain a base activator solution.
[0099] 4. The prepared powder mixture was mixed with the prepared alkali activator solution by using a constant temperature magnetic stirrer at room temperature, with a stirring speed of 180 r / min and a stirring time of 25 min to obtain a low-carbon resource utilization shield inert synchronous grouting material.
[0100] According to T-CECS 563-2018, GB / T1761-1999 and JGJ / T 70-2009, the performance of the low-carbon resource utilization shield inert synchronous grouting materials prepared in each embodiment and the shield inert synchronous grouting materials prepared in each comparative example were tested, as shown in Table 1:
[0101] Table 1. Properties of low-carbon resource utilization shield inert synchronous grouting materials
[0102]
[0103] From the data in the table, it can be seen that the 3d compressive strength of Examples 1 to 4 is 6.52 to 7.26 MPa, the 28d compressive strength is 19.56 to 21.69 MPa, the initial setting time is 3.5 to 6 hours, and the final setting time is 4.5 to 7 hours, which are all better than those of Comparative Examples 1 to 2, and are similar to the initial setting time and final setting time of Comparative Example 3 (containing cement), indicating that the low-carbon resource utilization shield inert synchronous grouting material prepared with a cement-free formula can achieve a setting time close to that of an active slurry (containing cement). In particular, the 3d compressive strength of Examples 1 to 4 is much higher than that of Comparative Examples 1 to 2, and is similar to the 3d compressive strength of Comparative Example 3 (containing cement), indicating that the low-carbon resource utilization shield inert synchronous grouting material prepared with a cement-free formula can achieve an early strength close to that of an active slurry (containing cement). According to the requirements of 3d compressive strength ≥ 0.5 and 28d compressive strength ≥ 2.5 in T-CECS563-2018, Examples 1 to 4 using the method of the present invention are far higher than the relevant mechanical property requirements in the specification. The consistency of Examples 1 to 4 is 9.2 to 10.2 cm. According to the requirement of 9 to 13 cm for the consistency of hydrated lime-based single-liquid synchronous grouting material in T-CECS563-2018, Examples 1 to 4 using the method of the present invention can meet the requirements and have good construction performance.
Claims
1. A low-carbon resource utilization shield inert synchronous grouting material, characterized in that: The raw materials include the following weight percentages: inert cementitious material 13%~20%, water 15.2%~19.5%, iron tailings sand 15%~20%, river sand 25%~31%, waste concrete 3%~4%, sodium bentonite 5%~6%, ultrafine powder of hot metal desulfurization slag 6%~7%, alkali activator 3%~4%, water reducer 0.2%~0.5%, admixture 1.5%~2.5%, and the total content of the above raw materials is 100%; The additive is a silane coupling agent composite solution, which is composed of the following components in percentage by mass: 25% silane coupling agent, 70% acetone and 5% water; The inert cementitious material is a mixture of silica fume, slag powder modified by an admixture, and kaolin modified by an admixture, wherein the mass ratio of slag powder, kaolin, and silica fume is (8-11): (3-5): (2-4).
2. A low-carbon resource utilization shield inert synchronous grouting material as claimed in claim 1, characterized in that: The effective components of the ultrafine powder of molten iron desulfurization slag are SO3, CaO, SiO2 and Al2O3, wherein the mass content of SO3 is 1.5%-2.5%, and the particle size grade of the ultrafine powder of molten iron desulfurization slag is 800 meshes.
3. A low-carbon resource utilization shield inert synchronous grouting material as claimed in claim 2, characterized in that: The particle size of the river sand is 0.2mm~0.5mm, the particle size of the iron tailings sand is 0.2mm~0.5mm, and the particle size of the waste concrete is 0.2mm~0.5mm.
4. A low-carbon resource utilization shield inert synchronous grouting material as claimed in claim 3, characterized in that: The water reducing agent is a powdered polycarboxylic acid high-efficiency water reducing agent.
5. A method for preparing a low-carbon resource utilization shield inert synchronous grouting material according to any one of claims 1 to 4, characterized in that: The preparation method is as follows: Step 1: Under the condition of 130° C. to 150° C., slag powder, metakaolin and iron tailings sand are separately mixed with the composite solution of the admixture silane coupling agent by magnetic stirring to obtain modified slag powder, modified metakaolin and modified iron tailings sand respectively; Step 2: Mixing the modified slag powder, modified metakaolin and silica fume at room temperature, and stirring with a constant temperature magnetic force to obtain an inert gelling material; Step 3: mixing inert cementitious material powder, modified iron tailings sand, river sand, waste concrete, sodium bentonite, ultrafine powder of molten iron desulfurization slag, and water reducing agent at room temperature to obtain a powder mixture; Step 4: Mixing the alkaline activator with water at room temperature, and stirring with a constant temperature magnetic force to obtain an alkaline activator solution; Step 5: Mix the powder mixture in step 3 with the alkaline activator solution in step 4, and stir them with a constant temperature magnetic force to obtain a low-carbon resource utilization shield inert synchronous grouting material.