A high wear-resistant and low friction polyethylene functional masterbatch and its preparation method and application
By adding ultra-high molecular weight polyethylene, talc and calcium carbonate to the polyethylene functional masterbatch, combined with zinc stearate and coupling agent, the problems of low wear resistance and high friction resistance of polyethylene sewage pipes are solved, and the problem of improved The material's wear resistance and sewage discharge effect.
Patent Information
- Application Number
- CN202211689095.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Polyethylene sewage pipes have low wear resistance and high friction resistance, which leads to easy blockage of the pipeline and short service life, affecting the sewage effect.
Using high wear-resistant and low friction resistance polyethylene functional masterbatch, the melting temperature difference is reduced and the wear resistance of the materials is enhanced by mixing ultra-high molecular weight polyethylene, talc powder and calcium carbonate, and using auxiliary materials such as zinc stearate and coupling agent. and self-lubricating properties, reducing friction resistance.
It significantly improves the wear resistance and toughness of polyethylene plastics, reduces the dynamic friction coefficient, extends the service life of the pipeline and improves the sewage discharge effect.
Smart Images

Figure BDA0004020522910000121 
Figure BDA0004020522910000131
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to a high-wear-resistant and low-friction polyethylene functional masterbatch and a preparation method and application thereof. Background Art
[0002] The sewage pipes on both sides of municipal roads, factories, units, and residential areas mainly include cement pipes, PVC (polyvinyl chloride), PE (polyethylene), PPR (polypropylene), and UPVC (rigid polyvinyl chloride) corrugated pipes, with a diameter of 0.05-2 meters, including rainwater pipes, sewage pipes, life and production pipes, and all pipes are circular pipes. At present, the focus of polyethylene sewage pipes is more on improving their rigidity and toughness.
[0003] However, in actual application, the impurities and sediment contained in the sewage in the pipe form mud, which scours and wears the inner wall of the pipe and affects the service life of the pipe. When the pressure in the pipe is not high and the flow rate is not high, the water flow in the pipe is small. Due to the large friction resistance of the pipe, it is easy to produce precipitation in the pipe, blocking the pipe, causing the pipe to be unable to be used normally, affecting the sewage discharge effect. In addition, the sewage pipes on both sides of the municipal highway are difficult to clear in time, resulting in sewage overflow, especially in the rainy season. The sewage pipes on both sides of the municipal highway are blocked, and the road surface of the community and the road surface are seriously waterlogged, resulting in water seepage in the basements of residential buildings and waterlogging on the road surface. For this reason, there are great losses of personnel and property.
[0004] Therefore, how to solve the problems of low wear resistance and high friction resistance of existing polyethylene sewage pipes and enhance the application functions of polyethylene sewage pipes has broad application prospects. Summary of the invention
[0005] The embodiments of the present application provide a highly wear-resistant and low-friction polyethylene functional masterbatch and a preparation method and application thereof, so as to solve the problems of low wear resistance and high friction resistance of polyethylene sewage pipes in the related art.
[0006] The technical solutions provided by this application are as follows:
[0007] In the first aspect, the present application provides a high wear-resistant and low friction polyethylene functional masterbatch, wherein the components are as follows by weight:
[0008] Ingredients:
[0009] 50 parts of polyethylene crushed material,
[0010] 10-20 parts of talcum powder,
[0011] Calcium carbonate 5-15 parts,
[0012] 10-20 parts of ultra-high molecular weight polyethylene material;
[0013] Excipients:
[0014] 1-3 parts of zinc stearate,
[0015] 2-4 parts of stearic acid,
[0016] 2-4 parts of coupling agent,
[0017] 1-3 parts of compatibilizer,
[0018] Dispersant 1-3 parts,
[0019] Antioxidant 0.5-1 part,
[0020] Masterbatch 0.5-1 part.
[0021] In some embodiments, the polyethylene crushed material includes one or more of waste recycled high-density polyethylene and waste recycled low-density polyethylene.
[0022] In some embodiments, the viscosity average molecular weight of the ultra-high molecular weight polyethylene material is 1.5-3 million, the particle size is 3-5 mm, and the viscosity number is 1200-1600 ml / g;
[0023] The viscosity average molecular weight of the polyethylene crushed material is 100,000-200,000.
[0024] In some embodiments, the coupling agent includes one or more of an aluminate coupling agent and a titanate coupling agent;
[0025] And / or, the compatibilizer includes an acrylate compatibilizer.
[0026] And / or, the dispersant comprises polyethylene wax.
[0027] And / or, the antioxidant comprises triphenyl phosphite.
[0028] In some embodiments, the masterbatch includes one or more of inorganic cadmium red, cadmium yellow, titanium dioxide, carbon black, red iron oxide, and yellow iron oxide.
[0029] In a second aspect, the present application also provides a method for preparing the high wear-resistant and low friction polyethylene functional masterbatch as described above, comprising the following steps:
[0030] The main material component and the auxiliary material component are mixed evenly to obtain a mixed material;
[0031] The mixed materials are sequentially extruded, cooled and pelletized through an extruder to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0032] In some embodiments, “mixing the main ingredient component and the auxiliary ingredient component uniformly” comprises the following steps:
[0033] Mix zinc stearate, stearic acid, coupling agent, compatibilizer, dispersant, antioxidant and masterbatch to form an auxiliary material package;
[0034] The polyethylene crushed material, talcum powder, calcium carbonate, ultra-high molecular weight polyethylene material and the auxiliary material package are kneaded in a closed mixer at a mixing temperature of 200-210° C. for 20-30 minutes.
[0035] In some embodiments, “mixing the main ingredient component and the auxiliary ingredient component uniformly” comprises the following steps:
[0036] Mix zinc stearate, stearic acid, coupling agent, antioxidant and masterbatch to form an auxiliary material package;
[0037] Premix talcum powder and calcium carbonate for 3-4 minutes, add the auxiliary material package and mix until the temperature reaches 100-110°C, add polyethylene crushed material, ultra-high molecular weight polyethylene material, compatibilizer and dispersant, mix evenly, and cool to 45-55°C.
[0038] In some embodiments, the barrel temperature of the extruder is set at 200-220°C, and the mold temperature is set at 190-200°C.
[0039] In a third aspect, the present application provides the use of the high wear-resistant and low friction polyethylene functional masterbatch as described above in the preparation of polyethylene plastics.
[0040] The beneficial effects of the technical solution provided by this application include:
[0041] (1) By mixing a certain amount of ultra-high molecular weight polyethylene into ordinary molecular weight polyethylene crushed materials, and using compatibilizers and zinc stearate to reduce the influence of melting temperature differences, the melt compatibility of two materials with different molecular weights is promoted, and the high wear resistance and self-lubricating properties of ultra-high molecular weight polyethylene "implanted" into ordinary low molecular weight polyethylene are achieved, thereby macroscopically improving the wear resistance of material products, reducing the dynamic friction coefficient, and reducing the friction resistance of material products;
[0042] (2) Talc and calcium carbonate are relatively cheap and have high hardness, which enhances the wear resistance and rigidity of the product and reduces the production cost. Adding coupling agent as the surface treatment agent of talc and calcium carbonate improves the interfacial bonding force between them and the organic polyethylene material, forms stress concentration points, changes the crystallinity and crystal area distribution of the polyethylene resin, and improves the strength and toughness of the product.
[0043] (3) Using stearic acid to perform surface activation treatment on talc and calcium carbonate, reduce the oil absorption value of inorganic substances, and promote the full and uniform dispersion of inorganic powders in the polyethylene matrix. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0045] In the first aspect, the embodiment of the present application provides a high wear-resistant and low friction polyethylene functional masterbatch, and the components are as follows by weight:
[0046] Ingredients:
[0047] 50 parts of polyethylene crushed material,
[0048] 10-20 parts of talcum powder,
[0049] Calcium carbonate 5-15 parts,
[0050] 10-20 parts of ultra-high molecular weight polyethylene material;
[0051] Excipients:
[0052] 1-3 parts of zinc stearate,
[0053] 2-4 parts of stearic acid,
[0054] 2-4 parts of coupling agent,
[0055] 1-3 parts of compatibilizer,
[0056] Dispersant 1-3 parts,
[0057] Antioxidant 0.5-1 part,
[0058] Masterbatch 0.5-1 part.
[0059] The present application achieves high wear resistance and self-lubricating properties of ultra-high molecular weight polyethylene "implanted" into ordinary low molecular weight polyethylene by mixing a certain amount of ultra-high molecular weight polyethylene into ordinary molecular weight polyethylene crushed materials, and reduces the influence of melting temperature difference by using compatibilizer and zinc stearate, thereby promoting the melting compatibility of two materials with different molecular weights, thereby macroscopically improving the wear resistance of material products, reducing the dynamic friction coefficient, and reducing the friction resistance of material products;
[0060] Talc and calcium carbonate are relatively low in price and high in hardness, which enhance the wear resistance and rigidity of the material products and reduce the production cost. Coupling agents are added as surface treatment agents for talc and calcium carbonate to improve their interfacial bonding with organic polyethylene materials, form stress concentration points, change the crystallinity and crystalline region distribution of polyethylene resins, and with the increase of molecular weight, the grain size decreases and the grain density increases, which directly affects the size change of the amorphous region. Under the condition of similar crystallinity, the thickness of the amorphous layer mainly bears the external energy absorption and conversion, that is, the increase in the thickness of the amorphous layer improves the strength and toughness of the material products. At the same time, the hardness of inorganic talc and calcium carbonate is relatively high, which improves the strength and toughness of the material products.
[0061] Stearic acid is used to perform surface activation treatment on talc and calcium carbonate to reduce the oil absorption value of inorganic substances and promote the inorganic powder to be fully and evenly dispersed in the polyethylene matrix.
[0062] In some embodiments, the polyethylene crushed material includes one or more of waste recycled high-density polyethylene and waste recycled low-density polyethylene.
[0063] By using clean recycled polyethylene material as the basic carrier material of the functional masterbatch, it is environmentally friendly and has good appearance and coagulation degree. Furthermore, the melt mass flow rate of the polyethylene crushed material is preferably 5-10g / 10min. As an example of polyethylene crushed material, such as linear low-density polyethylene recycled material.
[0064] In some embodiments, the ultra-high molecular weight polyethylene material has a viscosity average molecular weight of 1.5-3 million, a particle size of 3-5 mm, and a viscosity number of 1200-1600 ml / g;
[0065] The viscosity average molecular weight of the polyethylene crushed material is 100,000-200,000.
[0066] Furthermore, the ultra-high molecular weight polyethylene material is preferably a clean recycled material, so as to further improve the economic and environmental benefits of the functional masterbatch.
[0067] The present application uses low molecular weight polyethylene blended with high molecular weight polyethylene to ensure that the polyethylene plastic has sufficient rigidity and toughness while improving its wear resistance and reducing friction resistance.
[0068] In some embodiments, the talc powder is talc powder that has not been activated. Furthermore, the talc powder is 800-1000 mesh and has a uniform particle size.
[0069] In some embodiments, the calcium carbonate is heavy calcium carbonate that has not been activated, and further, the calcium carbonate is 1000-1200 mesh with uniform particle size;
[0070] In some embodiments, the coupling agent includes one or more of an aluminate coupling agent and a titanate coupling agent;
[0071] And / or, the compatibilizer includes an acrylate compatibilizer.
[0072] And / or, the dispersant comprises polyethylene wax.
[0073] And / or, the antioxidant comprises triphenyl phosphite.
[0074] Coupling agents are used for surface treatment of talcum powder and calcium carbonate to improve their interfacial bonding with organic polyethylene;
[0075] The compatibilizer is used to promote the melt compatibility of polyethylene crushed material and ultra-high molecular weight polyethylene material. Examples of the compatibilizer include methyl methacrylate, ACR resin (emulsified graft of acrylic monomer), etc.
[0076] The dispersant is used to improve the dispersion uniformity of each component. Furthermore, the polyethylene wax is prepared by a cracking method and has a melting point of 100-120°C;
[0077] Antioxidants are used to improve the weather resistance of polyethylene materials and extend their service life;
[0078] In some embodiments, the masterbatch includes one or more of inorganic cadmium red, cadmium yellow, titanium dioxide, carbon black, red iron oxide, and yellow iron oxide.
[0079] In some embodiments, the functional masterbatch may not contain zinc stearate, and the same effect can be achieved by increasing the amount of stearic acid added. For example, twice the amount of stearic acid as zinc stearate can be used to replace zinc stearate.
[0080] In some embodiments, industrial white oil 20# can also be used to replace stearic acid to achieve the same effect.
[0081] In a second aspect, the present application also provides a method for preparing the high wear-resistant and low friction polyethylene functional masterbatch as described above, comprising the following steps:
[0082] The main material component and the auxiliary material component are mixed evenly to obtain a mixed material;
[0083] The mixed materials are sequentially extruded, cooled and pelletized through an extruder to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0084] In some embodiments, the cooling method includes but is not limited to: crawler-type air cooling, water immersion cooling, forced air drying, etc.
[0085] In some embodiments, the pelletizing method includes but is not limited to: pelletizing by a pelletizer, water ring pelletizing, centrifugal drying, etc.
[0086] In some embodiments, the operation step of "extruder extrusion" includes:
[0087] The mixed material is added into the discharge port of the co-rotating twin-screw extruder and formed into a molten strand with a diameter of 3-5 mm through plasticization and extrusion.
[0088] In some embodiments, “mixing the main ingredient component and the auxiliary ingredient component uniformly” comprises the following steps:
[0089] Mix zinc stearate, stearic acid, coupling agent, compatibilizer, dispersant, antioxidant and masterbatch to form an auxiliary material package;
[0090] The polyethylene crushed material, talcum powder, calcium carbonate, ultra-high molecular weight polyethylene material and the auxiliary material package are kneaded in a closed mixer at a mixing temperature of 200-210° C. for 20-30 minutes.
[0091] In some embodiments, “mixing the main ingredient component and the auxiliary ingredient component uniformly” comprises the following steps:
[0092] Mix zinc stearate, stearic acid, coupling agent, antioxidant and masterbatch to form an auxiliary material package;
[0093] Premix talcum powder and calcium carbonate for 3-4 minutes, add the auxiliary material package and mix until the temperature reaches 100-110°C, add polyethylene crushed material, ultra-high molecular weight polyethylene material, compatibilizer and dispersant, mix evenly, and cool to 45-55°C.
[0094] In some embodiments, the barrel temperature of the extruder is set at 200-220°C, and the mold temperature is set at 190-200°C.
[0095] The preparation method provided in the present application can fully promote the compatibility and dispersibility between the main ingredients and improve the product quality.
[0096] In a third aspect, the present application provides the use of the high wear-resistant and low friction polyethylene functional masterbatch as described above in the preparation of polyethylene plastics.
[0097] The high-wear-resistant and low-friction polyethylene functional masterbatch provided in the present application can be used in combination with ordinary polyethylene production materials. The prepared polyethylene plastic has good rigidity, toughness, wear resistance and low friction, thereby improving the service life and use effect of the polyethylene sewage pipe.
[0098] The present application is further described below through specific examples.
[0099] Ingredients Description:
[0100] Polyethylene crushed material: high-density polyethylene and low-density polyethylene blended recycled clean material, the melt mass flow rate is 8-10g / 10min;
[0101] Talc: Type A 800-1000 mesh from Shouxin Mineral Products Processing Plant, Pailou Town, Haicheng, Liaoning;
[0102] Calcium carbonate: 1000-1200 mesh natural heavy calcium carbonate from Hangzhou Zhenghe Nanotechnology Co., Ltd.
[0103] Ultra-high molecular weight polyethylene material: Ultra-high molecular weight polyethylene recycled clean material, molecular weight 1.5 million-3 million;
[0104] Zinc stearate: Zhongshan Huamingtai Chemical Co., Ltd. brand BT2818;
[0105] Stearic acid: Malaysian type 1803;
[0106] Coupling agent: DL411 from Dongguan Dinghai Plastic Co., Ltd.;
[0107] Antioxidant: triphenyl phosphite TPPi from Zhangjiagang Yarui Chemical Co., Ltd.
[0108] Masterbatch: Chongqing Aocai New Materials Co., Ltd. T09294 black masterbatch;
[0109] Polyethylene production material: HDPE high-density polyethylene PE100 grade, PetroChina brand 7260.
[0110] Example 1
[0111] The present embodiment provides a high wear-resistant and low friction polyethylene functional masterbatch and a preparation method and application thereof.
[0112] (1) The preparation process of high wear-resistant and low friction polyethylene functional masterbatch is as follows:
[0113] 101: 1.5 parts of zinc stearate, 2 parts of stearic acid, 2 parts of coupling agent, 0.5 parts of antioxidant, and 0.5 parts of masterbatch are mixed to form an auxiliary material package;
[0114] 102: Add 15 parts of talcum powder and 10 parts of calcium carbonate into a high-speed mixer and premix for 3 minutes, add the auxiliary material package and continue high-speed mixing until the high-speed mixing temperature reaches 110°C, then discharge into a low-speed mixer, add 50 parts of polyethylene crushed material, 15 parts of ultra-high molecular weight polyethylene material, 1.5 parts of compatibilizer and 2 parts of dispersant, and cool the low-speed mixing to 55°C before discharging;
[0115] 103: adding the mixed material to the discharge port of the co-rotating twin-screw extruder, and forming a molten strand with a diameter of 3-5 mm through re-plasticization and extrusion. The barrel temperature of the co-rotating twin-screw extruder is set to 200-220° C., and the mold temperature is set to 190-200° C.;
[0116] 104: The extruded material is cooled by crawler air cooling and pelletized by a pelletizer to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0117] (2) Application of high wear-resistant and low friction polyethylene functional masterbatch:
[0118] The high wear-resistant and low friction polyethylene functional masterbatch prepared in step 104 is blended with the polyethylene production material in a mass ratio of 1:1 and 1:3 respectively, and sampled by a vulcanization tablet press to obtain polyethylene plastic, wherein the tablet pressing process is preheating at 180°C for 3 minutes, high pressure at 200°C for 15 minutes, and low pressure at 190°C for 10 minutes.
[0119] Example 2
[0120] The present embodiment provides a high wear-resistant and low friction polyethylene functional masterbatch and a preparation method and application thereof.
[0121] (1) The preparation process of high wear-resistant and low friction polyethylene functional masterbatch is as follows:
[0122] 101: 1.5 parts of zinc stearate, 2 parts of stearic acid, 2 parts of coupling agent, 0.5 parts of antioxidant, and 0.5 parts of masterbatch are mixed to form an auxiliary material package;
[0123] 102: Add 10 parts of talcum powder and 15 parts of calcium carbonate into a high-speed mixer and premix for 3 minutes, add the auxiliary material package and continue high-speed mixing until the high-speed mixing temperature reaches 110°C, then discharge into a low-speed mixer, add 50 parts of polyethylene crushed material, 15 parts of ultra-high molecular weight polyethylene material, 1.5 parts of compatibilizer and 2 parts of dispersant, cool the low-speed mixing to 55°C and discharge;
[0124] 103: adding the mixed material to the discharge port of the co-rotating twin-screw extruder, and forming a molten strand with a diameter of 3-5 mm through re-plasticization and extrusion. The barrel temperature of the co-rotating twin-screw extruder is set to 200-220° C., and the mold temperature is set to 190-200° C.;
[0125] 104: The extruded material is cooled by crawler air cooling and pelletized by a pelletizer to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0126] (2) Application of high wear-resistant and low friction polyethylene functional masterbatch:
[0127] The high wear-resistant and low friction polyethylene functional masterbatch prepared in step 104 is blended with the polyethylene production material in a mass ratio of 1:1 and 1:3 respectively, and sampled by a vulcanization tablet press to obtain polyethylene plastic, wherein the tablet pressing process is preheating at 180°C for 3 minutes, high pressure at 200°C for 15 minutes, and low pressure at 190°C for 10 minutes.
[0128] Example 3
[0129] The present embodiment provides a high wear-resistant and low friction polyethylene functional masterbatch and a preparation method and application thereof.
[0130] (1) The preparation process of high wear-resistant and low friction polyethylene functional masterbatch is as follows:
[0131] 101: Mix 1 part of zinc stearate, 2 parts of stearic acid, 2.5 parts of coupling agent, 0.5 parts of antioxidant, and 0.5 parts of masterbatch to form an auxiliary material package;
[0132] 102: Add 15 parts of talcum powder and 15 parts of calcium carbonate into a high-speed mixer and premix for 3 minutes, add the auxiliary material package and continue high-speed mixing until the high-speed mixing temperature reaches 110°C, then discharge into a low-speed mixer, add 50 parts of polyethylene crushed material, 10 parts of ultra-high molecular weight polyethylene material, 1 part of compatibilizer and 2.5 parts of dispersant, cool the low-speed mixing to 55°C and discharge;
[0133] 103: adding the mixed material to the discharge port of the co-rotating twin-screw extruder, and forming a molten strand with a diameter of 3-5 mm through re-plasticization and extrusion. The barrel temperature of the co-rotating twin-screw extruder is set to 200-220° C., and the mold temperature is set to 190-200° C.;
[0134] 104: The extruded material is cooled by crawler air cooling and pelletized by a pelletizer to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0135] (2) Application of high wear-resistant and low friction polyethylene functional masterbatch:
[0136] The high wear-resistant and low friction polyethylene functional masterbatch prepared in step 104 is blended with the polyethylene production material in a mass ratio of 1:1 and 1:3 respectively, and sampled by a vulcanization tablet press to obtain polyethylene plastic, wherein the tablet pressing process is preheating at 180°C for 3 minutes, high pressure at 200°C for 15 minutes, and low pressure at 190°C for 10 minutes.
[0137] Example 4
[0138] The present embodiment provides a high wear-resistant and low friction polyethylene functional masterbatch and a preparation method and application thereof.
[0139] (1) The preparation process of high wear-resistant and low friction polyethylene functional masterbatch is as follows:
[0140] 101: 2.5 parts of zinc stearate, 1 part of stearic acid, 3 parts of coupling agent, 0.5 parts of antioxidant, and 0.5 parts of masterbatch are mixed to form an auxiliary material package;
[0141] 102: Add 10 parts of talcum powder and 10 parts of calcium carbonate into a high-speed mixer and premix for 3 minutes, add the auxiliary material package and continue high-speed mixing until the high-speed mixing temperature reaches 110°C, then discharge into a low-speed mixer, add 50 parts of polyethylene crushed material, 20 parts of ultra-high molecular weight polyethylene material, 1 part of compatibilizer and 1.5 parts of dispersant, and cool the low-speed mixing to 55°C before discharging;
[0142] 103: adding the mixed material to the discharge port of the co-rotating twin-screw extruder, and forming a molten strand with a diameter of 3-5 mm through re-plasticization and extrusion. The barrel temperature of the co-rotating twin-screw extruder is set to 200-220° C., and the mold temperature is set to 190-200° C.;
[0143] 104: The extruded material is cooled by crawler air cooling and pelletized by a pelletizer to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
[0144] (2) Application of high wear-resistant and low friction polyethylene functional masterbatch:
[0145] The high wear-resistant and low friction polyethylene functional masterbatch prepared in step 104 is blended with the polyethylene production material in a mass ratio of 1:1 and 1:3 respectively, and sampled by a vulcanization tablet press to obtain polyethylene plastic, wherein the tablet pressing process is preheating at 180°C for 3 minutes, high pressure at 200°C for 15 minutes, and low pressure at 190°C for 10 minutes.
[0146] Comparative Example 1
[0147] This comparative example provides a polyethylene functional masterbatch and a preparation method and application thereof.
[0148] It includes most of the steps of Example 1, except that:
[0149] No talc added.
[0150] Comparative Example 2
[0151] This comparative example provides a polyethylene functional masterbatch and a preparation method and application thereof.
[0152] It includes most of the operations of Example 1, except that:
[0153] No calcium carbonate added.
[0154] Comparative Example 3
[0155] This comparative example provides a polyethylene functional masterbatch and a preparation method and application thereof.
[0156] It includes most of the operations of Example 1, except that:
[0157] No ultra high molecular weight polyethylene material is added.
[0158] Table 1: Formula ingredients of polyethylene functional masterbatch in various examples and comparative examples. (Unit: part)
[0159]
[0160] Note: "S" in Table 1 and Table 2 stands for "Example", for example: S1 refers to Example 1; "D" stands for "Comparative Example", for example: D1 refers to Comparative Example 1.
[0161] Performance Testing
[0162] The polyethylene plastics obtained in Examples 1-4 and Comparative Examples 1-3 were subjected to the following performance tests:
[0163] Wear rate: refer to SH / T 1818-2017;
[0164] Dynamic friction coefficient: GB10006-88 stipulates that the results are filled in Table 2.
[0165] Table 2
[0166]
[0167] In Table 2, the smaller the wear rate, the better the wear resistance, the smaller the dynamic friction coefficient, and the smaller the friction resistance. Combining the data of Examples 1-4 and the blank group, it can be seen that the polyethylene plastic added with the functional masterbatch provided by the present application has a wear rate reduced from 0.646% to below 0.5% and a dynamic friction coefficient reduced from 0.545 to below 0.4 compared with the existing ordinary polyethylene production material, indicating that the functional masterbatch provided by the present application can effectively improve the wear resistance of polyethylene plastics and reduce friction resistance;
[0168] Combined with the test results of Example 1, Comparative Example 3 and the blank group, compared with Example 1, Comparative Example 3 does not add ultra-high molecular weight polyethylene material, and its wear rate is above 0.6%, and its dynamic friction coefficient is above 0.5, which is not much different from the performance of ordinary production materials. In Example 1, by adding a certain amount of ultra-high molecular weight polyethylene material, the wear rate can be reduced to below 0.5%, and the dynamic friction coefficient can be reduced to below 0.4. This shows that the present application scheme can effectively improve the wear resistance of polyethylene plastics and reduce friction by adding ultra-high molecular weight polyethylene material.
[0169] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics, It is characterized in that The components are as follows by mass: Ingredients: 50 parts of polyethylene crushed material, 10-20 parts of talcum powder, Calcium carbonate 5-15 parts, 10-20 parts of ultra-high molecular weight polyethylene material; Excipients: 1-3 parts of zinc stearate, 2-4 parts of stearic acid, 2-4 parts of coupling agent, 1-3 parts of compatibilizer, Dispersant 1-3 parts, Antioxidant 0.5-1 part, Masterbatch 0.5-1 part; The coupling agent includes one or more of an aluminate coupling agent and a titanate coupling agent; The compatibilizer includes an acrylate compatibilizer; The polyethylene crushed material includes one or more of waste recycled high-density polyethylene and waste recycled low-density polyethylene.
2. The high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 1, It is characterized in that The ultra-high molecular weight polyethylene material has a viscosity average molecular weight of 1.5-3 million, a particle size of 3-5 mm, and a viscosity number of 1200-1600 ml / g; The viscosity average molecular weight of the polyethylene crushed material is 100,000-200,000.
3. The high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 1, It is characterized in that The dispersant includes polyethylene wax; And / or, the antioxidant comprises triphenyl phosphite.
4. The high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 1, It is characterized in that The color masterbatch includes one or more of inorganic cadmium red, cadmium yellow, titanium dioxide, carbon black, red iron oxide, and yellow iron oxide.
5. The method for preparing a high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to any one of claims 1 to 4, It is characterized in that The steps include: The main material component and the auxiliary material component are mixed evenly to obtain a mixed material; The mixed materials are sequentially extruded, cooled and pelletized through an extruder to obtain a high wear-resistant and low friction polyethylene functional masterbatch.
6. The method for preparing a high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 5, It is characterized in that "Uniformly mixing the main ingredient component and the auxiliary ingredient component" includes the following steps: Mix zinc stearate, stearic acid, coupling agent, compatibilizer, dispersant, antioxidant and masterbatch to form an auxiliary material package; The polyethylene crushed material, talcum powder, calcium carbonate, ultra-high molecular weight polyethylene material and the auxiliary material package are kneaded in a closed mixer at a mixing temperature of 200-210° C. for 20-30 minutes.
7. The method for preparing a high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 5, It is characterized in that "Uniformly mixing the main ingredient component and the auxiliary ingredient component" includes the following steps: Mix zinc stearate, stearic acid, coupling agent, antioxidant and masterbatch to form an auxiliary material package; Premix talcum powder and calcium carbonate for 3-4 minutes, add the auxiliary material package and mix until the temperature reaches 100-110°C, add polyethylene crushed material, ultra-high molecular weight polyethylene material, compatibilizer and dispersant, mix evenly, and cool to 45-55°C.
8. The method for preparing a high wear-resistant and low friction polyethylene functional masterbatch for preparing polyethylene plastics according to claim 5, It is characterized in that The barrel temperature of the extruder was set at 200-220°C, and the mold temperature was set at 190-200°C.