An epoxy resin-based copper powder conductive adhesive and aluminum electrode
By using epoxy resin-based copper powder conductive adhesive in aluminum electrodes, the adhesion ability of aluminum sheets is improved by using POSS composite materials and modified copper powder, the problems of short discharge time and potential fluctuations of aluminum electrodes are solved, and a longer time has been achieved discharge time and a more stable potential curve.
Patent Information
- Application Number
- CN202211684171.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The aluminum sheets are prone to fall off during the discharge process of existing aluminum electrodes, resulting in short discharge time and potential fluctuations, affecting the specific energy and stability of the battery.
Using an epoxy resin-based copper powder conductive glue, hydrolyzed with epoxy butyltrialkoxysilane containing 2 to 3 epoxy groups The POSS composite material prepared by the condensation reaction is modified copper powder, and the conductive glue is coated on the copper foil to improve the adhesion ability and discharge stability of the aluminum sheet.
It significantly extends the discharge time of the aluminum electrode, reduces the potential fluctuation during the discharge process, and improves the performance and stability of the aluminum electrode.
Smart Images

Figure HDA0004019197660000011 
Figure HDA0004019197660000012 
Figure HDA0004019197660000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum electrodes, and in particular to an epoxy resin-based copper powder conductive adhesive and an aluminum electrode prepared using the conductive adhesive. Background Art
[0002] The aluminum-air battery is composed of an aluminum electrode, an air electrode, and an electrolyte. It is a metal fuel cell with many advantages such as safety, cleanliness, non-toxicity, no emissions, and low price. It is an important development direction of green new energy. As the negative electrode of the aluminum-air battery, the aluminum electrode is a key factor in realizing the industrial application of aluminum-air batteries. The existing aluminum electrode is made of aluminum sheets and tabs connected by screws or welding. During the discharge process, the reaction speed on the surface of the aluminum sheet is uneven, and the reaction speed at the welding or screwing is fast, which makes it easy for the aluminum sheet and the tab to fall off. The detached aluminum sheet cannot continue to react to generate energy, resulting in a waste of raw materials and a decrease in the battery's specific energy.
[0003] The applicant provides an aluminum electrode in which an aluminum sheet is bonded to the surface of a copper foil in Chinese patent application 202010463193.X. Since the copper foil does not react in the electrolyte and will not corrode, preferential corrosion at the place where the aluminum sheet is bonded to the copper foil can be avoided. However, there are still problems such as premature detachment of the aluminum sheet resulting in a short discharge time and large potential fluctuations during the discharge process. After analysis, the inventor believes that this is mainly because the aluminum sheet is bonded to the copper foil through an epoxy resin conductive adhesive with copper powder as a conductive filler. Factors such as the conductive properties and bonding strength of the conductive adhesive affect the performance of the aluminum electrode. How to improve the performance of epoxy resin adhesive has become a technical problem that must be faced to improve the practical value of aluminum electrodes.
[0004] Wang Wenping et al. from Hefei University of Technology (Preparation and Performance Study of Polydisperse POSS / Epoxy Resin Composite Materials [J], New Chemical Materials, 2013.2, 41(2):36-38.) used 3-glycidyloxypropyltrimethoxysilane as raw material to synthesize polydisperse epoxy octasiloxane POSS-EP by silane hydrolysis method. Adding it to epoxy resin E-54 can improve the thermodynamic stability and mechanical properties of epoxy resin, providing an optional path to improve the performance of epoxy resin rubber. Summary of the invention
[0005] In view of the problem that the aluminum sheet still falls off and causes a short discharge time when the aluminum sheet is attached to the copper foil using copper powder conductive adhesive, the purpose of the present invention is to provide an epoxy resin-based copper powder conductive adhesive, which optimizes the composition of the copper powder conductive adhesive to improve the adhesion of the aluminum sheet to the copper foil, prolong the discharge time, and alleviate the potential fluctuation of the discharge process.
[0006] The present invention provides the following technical solutions:
[0007] An epoxy resin-based copper powder conductive adhesive comprises the following components in parts by weight:
[0008] 40-50 parts of epoxy resin, 50-60 parts of silane coupling agent modified copper powder, 5-7 parts of octasiloxane containing 2-3 epoxy groups, 2.7-3.5 parts of curing agent, and 8-12 parts of organic diluent;
[0009] The octasiloxane containing 2-3 epoxy groups is prepared by hydrolysis condensation reaction of ureapropyltrialkoxysilane and epoxybutyltrialkoxysilane in a molar ratio of 5-6:2-3, and the sum of the molar ratios of ureapropyltrialkoxysilane and epoxybutyltrialkoxysilane is 8.
[0010] Whether the conductive adhesive can meet the requirements of aluminum electrodes is not only related to the adhesive matrix, but also to the coordination of conductive fillers such as copper powder and the specific use scenarios. Its performance needs to be rigorously verified during the discharge process. The existing POSS composite epoxy resin usually only examines the performance of the composite material itself, without conductive fillers and discharge environment, which is quite different from the actual application scenario and cannot meet the actual application. The inventor team studied the application of conductive adhesive in aluminum electrodes and selected POSS composite epoxy resin containing 2 to 3 epoxy groups to improve the performance of epoxy resin, and prepared POSS by hydrolysis of ureapropyl trialkoxysilane and epoxybutyl trialkoxysilane. On the one hand, the number of epoxy groups in POSS is maintained at 2 to 3, avoiding excessive cross-linking caused by too many epoxy groups and the inability to effectively participate in cross-linking caused by too few epoxy groups; on the other hand, the introduction of ureapropyl improves the antioxidant protection of copper powder, and the carbon chain length of epoxybutyl trialkoxysilane is suitable, and the stability is also higher than the ether bond in glycidyloxypropyl trimethoxysilane. In this way, when the aluminum electrode is prepared by the conductive glue provided by the technical solution of the present application, the falling process of the aluminum sheet is delayed when the aluminum electrode is discharged, and the discharge time is significantly extended. At the same time, the time of the potential fluctuation during discharge is significantly postponed, and even basically no potential fluctuation occurs, which greatly improves the practical value of the aluminum electrode with an aluminum sheet / copper foil configuration.
[0011] As a preferred embodiment of the present invention, the silane coupling agent modified copper powder is obtained by dispersing the silane coupling agent in ethanol, adding copper powder, and drying after ultrasonic vibration. The amount of the silane coupling agent is 2-5% of the mass of the copper powder.
[0012] As the preferred embodiment of the present invention, the silane coupling agent used is ureapropyltrialkoxysilane. Although the use of the above-mentioned conductive glue can improve the discharge time of the aluminum electrode, the discharge stability of the aluminum electrode is not high, which is specifically manifested in that the discharge difference of the aluminum electrode of the same process is relatively large. After research, the inventor team believes that the main reason for this phenomenon is: in the copper powder conductive glue, the copper powder used is usually nanometer or micrometer level, and its particle size is generally above 20nm, while the molecular size of POSS is 1-2nm, which is much smaller than the size of the commonly used copper powder, which allows POSS to adhere to the surface of the copper powder and fill it between the copper powder and the copper powder and the epoxy resin. However, the substituents of POSS are epoxy and ureapropyl, which have low surface affinity with copper powder and unstable adhesion. Therefore, ureapropyltrialkoxysilane is selected to modify copper powder, and ureapropyl is introduced on the surface of copper powder, which is the same as the dominant substituent ureapropyl of POSS, which greatly improves the affinity of POSS to copper powder, so that the discharge consistency of the prepared aluminum electrode is improved.
[0013] As a preferred embodiment of the present invention, the ureapropyltrialkoxysilane is one or both of ureapropyltrimethylaminosilane and ureapropyltriethoxysilane.
[0014] As a preferred embodiment of the present invention, the epoxybutyl trialkoxysilane is one or both of epoxybutyl trimethoxysilane and epoxybutyl triethoxysilane.
[0015] As the preferred embodiment of the present invention, in the preparation process of the conductive adhesive, the epoxy resin is heated at 70-80° C. for 10-20 min, the octasil quioxane containing 2-3 epoxy groups is mixed with the silane coupling agent modified copper powder in ethanol, and then added to the epoxy resin for mixing, and then a mixture of a curing agent and an organic diluent is added for mixing, and the conductive adhesive is obtained by cooling. POSS is preferentially mixed with the modified copper powder to improve the adhesion of POSS to the copper powder, and then mixed with the epoxy resin, thereby improving the dispersion consistency of POSS and the copper powder and improving the process stability of the aluminum electrode preparation.
[0016] As a preference of the present invention, the curing agent is ethylenediamine, and / or the organic diluent is ethanol.
[0017] An aluminum electrode containing the copper powder conductive adhesive is prepared by uniformly coating the copper powder conductive adhesive on the surface of a clean copper foil, then laminating the clean aluminum sheet on the copper powder conductive adhesive, and curing the aluminum sheet at 80-85°C for 3-4 hours under 6-7MPa. The coating amount of the copper powder conductive adhesive is 2.5-4% of the total mass of the aluminum sheet and the copper foil.
[0018] As a preferred embodiment of the present invention,
[0019] The surface cleaning method of the aluminum sheet is as follows: soak the aluminum sheet in a sodium hydroxide or potassium hydroxide aqueous solution with a mass concentration of 10% to 20% at 50 to 60°C, wait for crystals to precipitate on the surface of the aluminum sheet, then take it out, rinse it, and dry it;
[0020] And / or, the surface cleaning method of the copper foil is: placing the copper foil in a degreasing liquid at 70-75° C. to remove grease, rinsing and drying after taking it out, then placing it in a rust removal liquid to remove copper rust, rinsing and drying after taking it out.
[0021] During storage, copper foil and aluminum foil will inevitably be oxidized, rusted or covered with oil film, which will seriously affect the bonding effect of the conductive glue and make it easy to fall off. At the same time, the oxide film of the aluminum foil will also cause the starting voltage of the battery to be too low, so the surface needs to be cleaned before use.
[0022] As a preferred embodiment of the present invention,
[0023] The composition of the degreasing liquid is: 10-20% Na2CO3, 10-20% NaH2PO4, 10-20% Na2SiO3, 2-3% OP emulsifier, and the balance is water;
[0024] The composition of the rust removal liquid is: 50%~55% H2SO4, 0.3%~0.5% HCl, 25%~30% HNO3, and the balance is water.
[0025] The beneficial effects of the present invention are as follows:
[0026] The present invention provides an epoxy resin-based copper powder conductive adhesive suitable for use in aluminum electrodes. By introducing octasilquioxane containing 2 to 3 epoxy groups to participate in the curing of the epoxy resin, the discharge time of the prepared aluminum electrode can be significantly increased, the volatility of the potential during the discharge process can be reduced, and the use performance of the aluminum electrode can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the potential curve of the aluminum electrode prepared in Example 1 during discharge.
[0028] Figure 2 This is a photograph of the aluminum electrode prepared in Example 1 after discharge.
[0029] Figure 3 This is a photograph of the aluminum electrode prepared in Example 4 after discharge.
[0030] Figure 4 This is a photograph of the aluminum electrode prepared in Example 5 after discharge.
[0031] Figure 5 This is a photograph of the aluminum electrode prepared in Example 6 after discharge.
[0032] Figure 6This is the potential curve of the aluminum electrode prepared in Comparative Example 1 during discharge.
[0033] Figure 7 This is a photograph of the aluminum electrode prepared in Comparative Example 1 after discharge.
[0034] Figure 8 This is a photograph of the aluminum electrode prepared in Comparative Example 2 after discharge.
[0035] Fig. 9 This is a photograph of the aluminum electrode prepared in Comparative Example 3 after discharge.
[0036] Fig.10 This is a photograph of the aluminum electrode prepared in Comparative Example 4 after discharge.
[0037] Fig.11 This is a photograph of the aluminum electrode prepared in Comparative Example 5 after discharge. DETAILED DESCRIPTION
[0038] The specific implementation modes of the present invention are further described below.
[0039] Unless otherwise specified, the raw materials used in the present invention can be purchased from the market or are commonly used in the art. Unless otherwise specified, the methods in the following embodiments are all conventional methods in the art.
[0040] Description of the test method for aluminum electrode performance:
[0041] The prepared aluminum electrode and air electrode were used to form an air battery, the electrolyte was potassium hydroxide (7 mol / L), and a closed-loop circuit was formed with a blue-electricity tester through a wire to charge the blue-electricity tester, and the potential changes of the aluminum electrode and the air electrode during the charging process of the blue-electricity tester were recorded;
[0042] The air electrode used is composed of a current collecting net, nickel foam, a catalytic layer waterproof and breathable membrane and an electrode ear, and the manufacturing method is as follows:
[0043] 1) Weld the current collector onto the nickel foam using a spot welder;
[0044] 2) Spraying catalyst on the combination of nickel foam and current collector
[0045] 3) Wrap the waterproof and breathable membrane on the side of the nickel foam sprayed with the catalytic layer and press them together using a press
[0046] 4) Use a spot welder to weld the pole ear on the oxygen electrode.
[0047] Example 1
[0048] An aluminum electrode is produced by the following process:
[0049] (1) Clean the surface of copper foil and aluminum sheet;
[0050] The surface cleaning process of copper foil is as follows:
[0051] The copper foil is degreased in a degreasing liquid at 70°C, the composition of which is: 10% Na2CO3, 20% NaH2PO4, 20% Na2SiO3, 3% OP emulsifier, and the balance is water; after being taken out, it is rinsed and dried; then the copper foil is placed in a rust removal liquid to remove rust, the composition of which is: 50% H2SO4, 0.5% HCl, 30% HNO3, and the balance is water; after rust removal, the copper foil is rinsed and dried on an iron plate at 100°C;
[0052] The surface cleaning process of aluminum sheet is as follows:
[0053] The aluminum sheet was immersed in a 10% sodium hydroxide aqueous solution at 60°C. After crystals were precipitated on the surface of the aluminum sheet, it was taken out, rinsed, and dried on an iron plate at 100°C.
[0054] (2) Preparation of copper powder conductive adhesive;
[0055] Step 1: dispersing 3-glycidyloxypropyltrimethoxysilane in ethanol and dissolving it, then dispersing copper powder with a particle size of 40 nm in ethanol, ultrasonically treating for 45 minutes, and then drying and removing ethanol to obtain silane coupling agent modified copper powder, the amount of 3-glycidyloxypropyltrimethoxysilane used is 3% of the mass of the copper powder;
[0056] Step 2: Heat anhydrous ethanol to 40°C, add deionized water and hydrochloric acid under reflux, stir evenly and then drop ureapropyl trimethoxysilane and epoxybutyl trimethoxysilane, and hydrolyze for 72 hours after the addition is complete. The molar ratio of ureapropyl trimethoxysilane to epoxybutyl trimethoxysilane is 5:3, and the molar ratio of water to total silane is 3:1. After the reaction, adjust the system to neutral, remove the solvent, dry and filter to obtain octasiloxane substituted with epoxy and ureapropyl groups;
[0057] Step 3: Take 40 parts by weight of epoxy resin E-51 and heat it to 80°C for preheating for 10 minutes, add 8 parts of ethanol and stir evenly, add 60 parts of silane coupling agent modified copper powder prepared in step 1 and stir evenly, then add 5 parts of octasiloxane POSS prepared in step 2 and stir evenly, then add 2.7 parts of curing agent ethylenediamine and stir evenly to obtain copper powder conductive adhesive;
[0058] (3) Coating the copper powder conductive adhesive prepared in step (2) on the copper foil with an area equal to that of the aluminum sheet, wherein the coating amount of the copper powder conductive adhesive is 3% of the total mass of the copper foil and the aluminum sheet, and then laminating the aluminum sheet on the copper powder conductive adhesive, and then pressing at a pressure of 6 MPa for 3 h at a pressing temperature of 80° C. to achieve the curing of the copper powder conductive adhesive to obtain an aluminum electrode.
[0059] The aluminum electrode prepared in this embodiment and the air electrode were used to form an air battery and then discharged. The blue electric tester was charged to record the potential change of the aluminum electrode during the discharge process. The obtained potential curve is as follows: Figure 1 As shown in the figure, the potential of the aluminum electrode began to increase 48 minutes after the start of the experiment. The experiment was stopped 53 minutes later. After the aluminum electrode was taken out, it was found that the aluminum sheet and the copper foil did not fall off. Figure 2 The process of Example 1 was repeated to prepare two more groups of aluminum electrodes for testing. The time when the potential began to increase was 42 minutes and 50 minutes respectively, and no electrode fell off when the experiment was stopped at 53 minutes.
[0060] Example 2
[0061] An aluminum electrode is produced by the following process:
[0062] (1) Clean the surface of copper foil and aluminum sheet;
[0063] The surface cleaning process of copper foil is as follows:
[0064] The copper foil was placed in a degreasing liquid at 70°C to remove grease. The composition of the degreasing liquid used was: 20% Na2CO3, 10% NaH2PO4, 15% Na2SiO3, 2% OP emulsifier, and the balance was water. After taking it out, it was rinsed and dried. Then the copper foil was placed in a rust removal liquid to remove rust. The composition of the rust removal liquid used was: 55% H2SO4, 0.3% HCl, 25% HNO3, and the balance was water. After rust removal, the copper foil was rinsed and dried on an iron plate at 100°C.
[0065] The surface cleaning process of aluminum sheet is as follows:
[0066] At 60°C, immerse the aluminum sheet in a 20% sodium hydroxide aqueous solution. After crystals precipitate on the surface of the aluminum sheet, take it out, rinse it, and dry it on an iron plate at 100°C.
[0067] (2) Preparation of copper powder conductive adhesive;
[0068] Step 1: dispersing 3-glycidyloxypropyltrimethoxysilane in ethanol and dissolving it, then dispersing copper powder with a particle size of 40 nm in ethanol, ultrasonically treating for 45 minutes, and then drying and removing ethanol to obtain silane coupling agent modified copper powder, the amount of 3-glycidyloxypropyltrimethoxysilane used is 5% of the mass of the copper powder;
[0069] Step 2: Heat anhydrous ethanol to 40°C, add deionized water and hydrochloric acid under reflux, stir evenly and then drop ureapropyl trimethoxysilane and epoxybutyl trimethoxysilane, and hydrolyze for 72 hours after the addition is complete. The molar ratio of ureapropyl trimethoxysilane to epoxybutyl trimethoxysilane is 6:2, and the molar ratio of water to total silane is 3:1. After the reaction, adjust the system to neutral, remove the solvent, dry and filter to obtain octasiloxane substituted with epoxy and ureapropyl groups;
[0070] Step 3: Take 50 parts by weight of epoxy resin E-51 and heat it to 80°C for preheating for 10 minutes, add 12 parts of ethanol and stir evenly, then add 50 parts of silane coupling agent modified copper powder prepared in step 1 and stir evenly, then add 7 parts of octasiloxane POSS prepared in step 2 and stir evenly, then add 3.5 parts of curing agent ethylenediamine and stir evenly to obtain copper powder conductive adhesive;
[0071] (3) Coating the copper powder conductive adhesive prepared in step (2) on the copper foil in an area equal to that of the aluminum sheet, wherein the coating amount of the copper powder conductive adhesive is 4% of the total mass of the copper foil and the aluminum sheet, and then laminating the aluminum sheet on the copper powder conductive adhesive, and then pressing at a pressure of 6 MPa for 3 h at a pressing temperature of 80° C. to achieve curing of the copper powder conductive adhesive.
[0072] The process of this embodiment was repeated to prepare 3 groups of aluminum electrodes, which were respectively combined with air electrodes to form air batteries and then discharged. The blue battery tester was charged and the potential changes of the aluminum electrodes during the discharge process were recorded. The time when the potential of each group of electrodes began to increase was 42, 46, and 51 minutes, respectively. The test was automatically stopped after 55 minutes. After taking out the aluminum electrodes, it was found that the aluminum sheet and the copper foil had not fallen off.
[0073] Example 3
[0074] An aluminum electrode is produced by the following process:
[0075] (1) Clean the surface of copper foil and aluminum sheet;
[0076] The surface cleaning process of copper foil is as follows:
[0077] The copper foil was placed in a degreasing liquid at 70°C to remove grease. The composition of the degreasing liquid used was: 15% Na2CO3, 15% NaH2PO4, 15% Na2SiO3, 3% OP emulsifier, and the balance was water. After taking it out, it was rinsed and dried. Then the copper foil was placed in a rust removal liquid to remove rust. The composition of the rust removal liquid used was: 50% H2SO4, 0.5% HCl, 25% HNO3, and the balance was water. After rust removal, the copper foil was rinsed and dried on an iron plate at 100°C.
[0078] The surface cleaning process of aluminum sheet is as follows:
[0079] At 60°C, immerse the aluminum sheet in a 10% sodium hydroxide solution. After crystals precipitate on the surface of the aluminum sheet, take it out, rinse it, and dry it on an iron plate at 100°C.
[0080] (2) Preparation of copper powder conductive adhesive;
[0081] Step 1: dispersing 3-glycidyloxypropyltrimethoxysilane in ethanol and dissolving it, then dispersing copper powder with a particle size of 40 nm in ethanol, ultrasonically treating for 45 minutes, and then drying and removing ethanol to obtain silane coupling agent modified copper powder, the amount of 3-glycidyloxypropyltrimethoxysilane used is 2% of the mass of the copper powder;
[0082] Step 2: Heat anhydrous ethanol to 40°C, add deionized water and hydrochloric acid under reflux, stir evenly and then drop ureapropyl trimethoxysilane and epoxybutyl trimethoxysilane, and hydrolyze for 72 hours after the addition is complete. The molar ratio of ureapropyl trimethoxysilane to epoxybutyl trimethoxysilane is 5:3, and the molar ratio of water to total silane is 3:1. After the reaction, adjust the system to neutral, remove the solvent, dry and filter to obtain octasiloxane substituted with epoxy and ureapropyl groups;
[0083] Step 3: Take 45 parts by weight of epoxy resin E-51 and heat it to 80°C for preheating for 10 minutes, add 10 parts of ethanol and stir evenly, then add 55 parts of silane coupling agent modified copper powder prepared in step 1 and stir evenly, then add 6 parts of octasilane quioxane POSS prepared in step 2 and stir evenly, add 3 parts of curing agent ethylenediamine and stir evenly to obtain copper powder conductive adhesive;
[0084] (3) Coating the copper powder conductive adhesive prepared in step (2) on the copper foil in an area equal to that of the aluminum sheet, wherein the coating amount of the copper powder conductive adhesive is 2.5% of the total mass of the copper foil and the aluminum sheet, and then laminating the aluminum sheet on the copper powder conductive adhesive, and then pressing at a pressure of 6 MPa for 3 h at a pressing temperature of 80° C. to achieve curing of the copper powder conductive adhesive.
[0085] The process of this embodiment was repeated to prepare 3 groups of aluminum electrodes, which were respectively formed into air batteries with air electrodes and discharged. The blue battery tester was charged and the potential change of the aluminum electrodes during the discharge process was recorded. The time when the potential of each group of electrodes began to increase was 44, 49, and 52 minutes, respectively. The test was stopped after 55 minutes, and the aluminum sheet and copper foil did not fall off.
[0086] Example 4
[0087] An aluminum electrode, which is different from Example 1 in that:
[0088] When preparing the copper powder conductive adhesive in step (2), ureapropyl trimethylsiloxane is used to prepare the silane coupling agent modified copper powder.
[0089] The aluminum electrode prepared in this embodiment and the air electrode were used to form an air battery and then discharged. The blue electric tester was charged to record the potential change of the aluminum electrode during the discharge process. The potential of the first group of aluminum electrodes increased 60 minutes after the start of the test, and the experiment was stopped after 61 minutes. After the aluminum electrode was taken out, the aluminum sheet and the copper foil did not fall off. Figure 3 The process of this embodiment was repeated to prepare two more groups of aluminum electrodes for testing. The potential increase time was 56 minutes and 59 minutes respectively. When the test was stopped at 62 minutes, no electrode fell off.
[0090] Example 5
[0091] An aluminum electrode, which is different from Example 1 in that:
[0092] When preparing the copper powder conductive adhesive in step (2), in step 3, the silane coupling agent-modified copper powder and the octasiloxane quioxane POSS are stirred evenly in ethanol and then added to the epoxy resin E-51, and then the curing agent ethylenediamine is added.
[0093] The aluminum electrode prepared in this embodiment and the air electrode were used to form an air battery and then discharged. The blue electric tester was charged to record the potential change of the aluminum electrode during the discharge process. The potential of the first group of aluminum electrodes increased 58 minutes after the start of the test, and the experiment was stopped after 61 minutes. After the aluminum electrode was taken out, the aluminum sheet and the copper foil did not fall off. Figure 4 The process of this embodiment was repeated to prepare two more groups of aluminum electrodes for testing. The potential increase time was 55min and 53min respectively, and no electrode fell off when the test was stopped at 62min.
[0094] Example 6
[0095] An aluminum electrode, which is different from Example 1 in that:
[0096] When preparing the copper powder conductive adhesive in step (2), ureapropyl trimethylsiloxane is used to prepare the silane coupling agent modified copper powder.
[0097] When preparing the copper powder conductive adhesive in step (2), in step 3, the silane coupling agent-modified copper powder and the octasiloxane quioxane POSS are stirred evenly in ethanol and then added to the epoxy resin E-51, and then the curing agent ethylenediamine is added.
[0098] The aluminum electrode prepared in this embodiment and the air electrode were used to form an air battery and then discharged. The blue electric tester was charged to record the potential change of the aluminum electrode during the discharge process. The potential of the first group of aluminum electrodes increased 62 minutes after the start of the test, and the experiment was stopped after 61 minutes. After the aluminum electrode was taken out, the aluminum sheet and the copper foil did not fall off. Figure 5 The process of this embodiment was repeated to prepare two more groups of aluminum electrodes for testing, and the potential increase time was 61min and 60min respectively, and no electrode fell off when the test was stopped at 64min.
[0099] Comparative Example 1
[0100] The difference from Example 1 is that the prepared epoxy octasilquioxane POSS is not added during the preparation of the aluminum electrode.
[0101] The aluminum electrode is used to form an air battery and then charged with a blue electric tester to test its performance. The potential curve of the aluminum electrode during the discharge process is as follows: Figure 6 As shown in Figure 1, at 8 minutes after the start of the test, the potential of the aluminum electrode suddenly began to fluctuate greatly. After 9 minutes, the experiment was stopped and the aluminum sheet fell off after the aluminum electrode was taken out. Figure 7 shown.
[0102] Comparative Example 2
[0103] The difference from Example 1 is that the octasilquioxane used is prepared by the hydrolysis condensation reaction of 3-glycidyloxypropyltrimethoxysilane.
[0104] The aluminum electrode was used to form an air battery and then charged with a blue electric tester to test its performance. As shown in the figure, the potential of the aluminum electrode fluctuated after 7 minutes, stabilized after 9 minutes, and began to fluctuate again after 21 minutes. The experiment was stopped after 22 minutes. After the aluminum electrode was taken out, the aluminum sheet and the copper foil fell off. Figure 8 shown.
[0105] Comparative Example 3
[0106] The difference from Example 1 is that when preparing octasilquioxane POSS, 3-glycidyloxypropyltrimethoxysilane is used instead of epoxybutyltrimethoxysilane.
[0107] The aluminum electrode was used to form an air battery and then charged with a blue electric tester to test its performance. The potential of the aluminum electrode gradually increased after 30 minutes. The experiment was stopped after 39 minutes. After the aluminum electrode was taken out, the aluminum sheet fell off. Fig. 9 shown.
[0108] Comparative Example 4
[0109] The difference from Example 1 is that KH550 is used instead of ureapropyltrimethoxysilane.
[0110] The aluminum electrode was assembled into an air battery and then charged with a blue electric tester to test its performance. The potential of the aluminum electrode gradually increased after 23 minutes. The experiment was stopped after 25 minutes. After the aluminum electrode was taken out, the aluminum sheet fell off. Fig.10 shown.
[0111] Comparative Example 5
[0112] The difference from Example 1 is that when preparing the octasilquioxane POSS, the molar ratio of ureapropyltrimethoxysilane to epoxybutyltrimethoxysilane is 7:1.
[0113] The aluminum electrode was assembled into an air battery and then charged with a blue electric tester to test its performance. The potential of the aluminum electrode gradually increased after 12 minutes. The experiment was stopped after 15 minutes. After the aluminum electrode was taken out, the aluminum sheet fell off. Fig.11 shown.
[0114] It can be seen from the test results of the above embodiments and comparative examples that the aluminum electrode prepared by the technical solution of the present application has a longer discharge time, low discharge volatility, and will not fall off during the test time.
Claims
1. An epoxy resin-based copper powder conductive adhesive, characterized in that: The composition comprises the following components in parts by weight: 40-50 parts of epoxy resin, 50-60 parts of silane coupling agent modified copper powder, 5-7 parts of octasiloxane containing 2-3 epoxy groups, 2.7-3.5 parts of curing agent, and 8-12 parts of organic diluent; The octasiloxane containing 2-3 epoxy groups is prepared by hydrolysis condensation reaction of ureapropyltrialkoxysilane and epoxybutyltrialkoxysilane in a molar ratio of 5-6:2-3, and the sum of the molar ratios of ureapropyltrialkoxysilane and epoxybutyltrialkoxysilane is 8.
2. The epoxy resin-based copper powder conductive adhesive according to claim 1, characterized in that: The silane coupling agent modified copper powder is obtained by dispersing the silane coupling agent in ethanol, adding the copper powder, and drying after ultrasonic vibration. The amount of the silane coupling agent used is 2% to 5% of the mass of the copper powder.
3. The epoxy resin-based copper powder conductive adhesive according to claim 2, characterized in that: The silane coupling agent used is ureapropyltrialkoxysilane.
4. The epoxy resin-based copper powder conductive adhesive according to claim 1, 2 or 3, characterized in that: The ureapropyl trialkoxysilane is one or both of ureapropyl trimethoxysilane and ureapropyl triethoxysilane.
5. The epoxy resin-based copper powder conductive adhesive according to claim 1, characterized in that: The epoxybutyl trialkoxysilane is one or both of epoxybutyl trimethoxysilane and epoxybutyl triethoxysilane.
6. The epoxy resin-based copper powder conductive adhesive according to claim 1, 2 or 3, characterized in that: In the preparation process of the conductive adhesive, the epoxy resin is heated at 70-80° C. for 10-20 minutes, octasil quioxane containing 2-3 epoxy groups and silane coupling agent modified copper powder are mixed in ethanol, added to the epoxy resin and mixed, and then a mixture of a curing agent and an organic diluent is added and mixed, and the conductive adhesive is obtained by cooling.
7. The epoxy resin-based copper powder conductive adhesive according to claim 1, characterized in that: The curing agent is ethylenediamine, and / or the organic diluent is ethanol.
8. An aluminum electrode containing the copper powder conductive paste according to any one of claims 1 to 7, characterized in that: Copper powder conductive adhesive is evenly coated on the clean surface of copper foil, and then the clean surface of aluminum sheet is attached to the copper powder conductive adhesive, and cured at 80-85°C for 3-4 hours under 6-7Mpa.
9. The aluminum electrode according to claim 8, characterized in that The surface cleaning method of the aluminum sheet is as follows: soak the aluminum sheet in a sodium hydroxide or potassium hydroxide aqueous solution with a mass concentration of 10% to 20% at 50 to 60°C, wait for crystals to precipitate on the surface of the aluminum sheet, then take it out, rinse it, and dry it; And / or, the surface cleaning method of the copper foil is: placing the copper foil in a degreasing liquid at 70-75° C. to remove grease, rinsing and drying after taking it out, then placing it in a rust removal liquid to remove copper rust, rinsing and drying after taking it out.
10. The aluminum electrode according to claim 8, characterized in that The composition of the degreasing liquid is: 10-20% Na2CO3, 10-20% NaH2PO4, 10-20% Na2SiO3, 2-3% OP emulsifier, and the balance is water; The composition of the rust removal liquid is: 50%~55% H2SO4, 0.3%~0.5% HCl, 25%~30% HNO3, and the balance is water.