A high-stamping automobile aluminum alloy body panel material and preparation method thereof
By combining hollow ceramic membranes with aluminum alloys and reinforcing with titanium diboride particles, the problem of insufficient stamping resistance of aluminum alloy body panels was solved, and the mechanical properties of high-stampability automotive aluminum alloy body panels were improved.
Patent Information
- Application Number
- CN202211661779.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Existing aluminum alloy body panel materials are insufficient in terms of mechanical properties such as stamping resistance and elongation, making it difficult to meet the requirements of high stamping performance.
A hollow ceramic membrane is used as the overall support structure and combined with aluminum alloy. The hollow ceramic membrane is made by electrospinning and combined with titanium diboride particles as a reinforcing material. The microstructure of the aluminum alloy is improved by homogenization treatment to prepare high-stampability automotive aluminum alloy body panel material.
It improves the compressive strength and elongation of the material, compensates for the brittleness of ceramic materials, enhances the mechanical properties of aluminum alloys, and improves the stamping properties of automobile body panels.
Abstract
Description
Technical Field
[0001] The invention relates to the field of alloy materials, and in particular to a high-stamping automobile aluminum alloy body panel material and a preparation method thereof. Background Art
[0002] The world's automobile industry is facing three increasingly severe problems: energy, environment, and safety. Therefore, reducing the weight of the car to reduce energy consumption, reduce pollution, and improve efficiency has become an important measure for major automobile manufacturers to improve their competitiveness. For every 100kg reduction in the weight of the car, the fuel consumption can be reduced by 0.7L / km. At present, the use of aluminum alloy instead of steel is the main weight reduction measure for automobile manufacturers in various countries. To achieve the same mechanical performance indicators, aluminum is 60% lighter than steel. Replacing traditional steel plates with aluminum alloys on the inner and outer panels of the car can reduce the weight of the entire vehicle by about 47%. Under the same impact, aluminum plates absorb 50% more impact energy than steel plates. Aluminum alloy cars are also favored for their energy saving and consumption reduction, environmental protection, high recycling rate of aluminum alloy parts, safety and comfort, reduced processes, high assembly efficiency, high fuel efficiency, and large relative load capacity. The car body is the heaviest part of the car, accounting for about 30% of the total weight of the car. Therefore, aluminum alloy has become the choice of 99% of automobile body panels. However, aluminum alloy also has certain mechanical property defects, such as poor stamping resistance, compression resistance and elongation. Therefore, the modification of aluminum alloy materials has become a top priority. Summary of the invention
[0003] Technical problem to be solved: The purpose of the present invention is to provide a high-stamping automotive aluminum alloy body panel material. By adopting a hollow ceramic membrane as the overall supporting structure, the ceramic has the advantages of high melting point, high hardness, high wear resistance, oxidation resistance, etc. As the supporting structure of the body panel, it can improve the material's compressive resistance, elongation and other mechanical properties; at the same time, the ceramic membrane used is hollow, and after the aluminum alloy is poured into the mold, it will also flow into the ceramic membrane tube to compensate for the brittleness of the ceramic material.
[0004] Technical solution: A high-stamping automotive aluminum alloy body panel material, which is composed of a ceramic film and an aluminum alloy. The hollow ceramic film is made by an electrostatic spinning method. The reinforced aluminum alloy is composed of an aluminum alloy substrate and reinforced particles. The aluminum alloy substrate includes the following components:
[0005] Si is 0.2-1.0%;
[0006] Mg: 0.5-1.5%;
[0007] Zn: 0.2- 0.5%;
[0008] Ce: 0.2-0.35%
[0009] The balance is Al.
[0010] Preferably, the porosity of the hollow ceramic membrane is 20-40%.
[0011] Preferably, the preparation method of the hollow ceramic membrane is as follows:
[0012] S1: Take yttrium zirconium oxide powder, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone, mix and stir for 24 hours to obtain a spinning solution;
[0013] S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05 MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 15-20 ml / min. After passing through an air gap of 1.5 cm, the two enter the water and gel into a hollow fiber membrane;
[0014] S3: drying the solidified hollow fiber membrane at room temperature for 24 h;
[0015] S4: Raise the temperature to 700°C at a rate of 2°C / min and keep it at that temperature for 2 h, then raise the temperature to 1320°C at a rate of 5°C / min and keep it at that temperature for 5 h. Naturally cool to room temperature to obtain a hollow ceramic membrane.
[0016] Preferably, the yttrium-doped zirconium oxide powder has a D50 of 0.80 μm.
[0017] Preferably, the mass ratio of the yttrium-doped zirconium oxide, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0.
[0018] Preferably, the diameters of the inner tube and outer tube of the nozzle in the electrostatic device are 2.5 mm and 1.0 mm respectively.
[0019] Preferably, the reinforcing particles are titanium diboride particles, and the addition amount is 5-10wt.% of the aluminum alloy.
[0020] Preferably, the particle size of the titanium diboride particles is 1-20 μm.
[0021] The preparation method of the above-mentioned automobile aluminum alloy body plate material comprises the following steps:
[0022] Step 1: Place the aluminum alloy substrate and the reinforced particles in a heat treatment furnace and perform homogenization treatment at a temperature of 440-450° C. for 25-30 hours to obtain a reinforced aluminum alloy;
[0023] Step 2: Place the hollow ceramic membrane in a body panel mold, pour the reinforced aluminum alloy into the mold, and cool it naturally in the air.
[0024] Preferably, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:(3-5).
[0025] Beneficial effects:
[0026] 1. The present invention adopts hollow ceramic membrane as the overall supporting structure. Ceramics have the advantages of high melting point, high hardness, high wear resistance, oxidation resistance, etc. As the supporting structure of the body panel, it can improve the material's compressive resistance, elongation and other mechanical properties.
[0027] 2. The ceramic membrane used in the present invention is hollow. After the aluminum alloy is poured into the mold, it will also flow into the ceramic membrane tube to compensate for the brittleness of the ceramic material.
[0028] 3. The present invention uses titanium diboride particles as a reinforcing material. The addition of titanium diboride particles can reduce the average phase spacing of the non-equilibrium eutectic phase in the aluminum alloy structure, thereby shortening the element diffusion time. After homogenization treatment, the non-equilibrium eutectic phase in the aluminum alloy material structure is basically eliminated, the problem of high brittleness is solved, and the mechanical properties are enhanced. DETAILED DESCRIPTION
[0029] The present invention proposes a high stamping performance automotive aluminum alloy body panel material and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention will be further described in detail with reference to the embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Example
[0030] The preparation method of hollow ceramic membrane is as follows:
[0031] S1: Yttrium-doped zirconium oxide powder, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone are mixed and stirred for 24 hours to obtain a spinning solution; wherein the yttrium-doped zirconium oxide powder D50=0.80μm; the mass ratio of the yttrium-doped zirconium oxide, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0;
[0032] S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05 MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 15 ml / min. After passing through an air gap of 1.5 cm, the two enter the water and gel into a hollow fiber membrane. Among them, the diameters of the inner tube and outer tube of the nozzle in the electrostatic device are 2.5 mm and 1.0 mm respectively.
[0033] S3: drying the solidified hollow fiber membrane at room temperature for 24 h;
[0034] S4: Raise the temperature to 700°C at a rate of 2°C / min and keep it at that temperature for 2 h, then raise the temperature to 1320°C at a rate of 5°C / min and keep it at that temperature for 5 h. Naturally cool to room temperature to obtain a hollow ceramic membrane.
[0035] The porosity of the hollow ceramic membrane is 37.2%. Example
[0036] The preparation method of hollow ceramic membrane is as follows:
[0037] S1: Yttrium-doped zirconium oxide powder, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone are mixed and stirred for 24 hours to obtain a spinning solution; wherein the yttrium-doped zirconium oxide powder D50=0.80μm; the mass ratio of the yttrium-doped zirconium oxide, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0;
[0038] S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05 MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 17 ml / min. After passing through an air gap of 1.5 cm, the two enter the water and gel into a hollow fiber membrane. Among them, the diameters of the inner tube and outer tube of the nozzle in the electrostatic equipment are 2.5 mm and 1.0 mm respectively.
[0039] S3: drying the solidified hollow fiber membrane at room temperature for 24 h;
[0040] S4: Raise the temperature to 700°C at a rate of 2°C / min and keep it at that temperature for 2 h, then raise the temperature to 1320°C at a rate of 5°C / min and keep it at that temperature for 5 h. Naturally cool to room temperature to obtain a hollow ceramic membrane.
[0041] The porosity of the hollow ceramic membrane is 33.4%. Example
[0042] The preparation method of hollow ceramic membrane is as follows:
[0043] S1: Yttrium-doped zirconium oxide powder, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone are mixed and stirred for 24 hours to obtain a spinning solution; wherein the yttrium-doped zirconium oxide powder D50=0.80μm; the mass ratio of the yttrium-doped zirconium oxide, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0;
[0044] S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05 MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 18 ml / min. After passing through an air gap of 1.5 cm, the two enter the water and gel into a hollow fiber membrane. Among them, the diameters of the inner tube and outer tube of the nozzle in the electrostatic device are 2.5 mm and 1.0 mm respectively.
[0045] S3: drying the solidified hollow fiber membrane at room temperature for 24 h;
[0046] S4: Raise the temperature to 700°C at a rate of 2°C / min and keep it at that temperature for 2 h, then raise the temperature to 1320°C at a rate of 5°C / min and keep it at that temperature for 5 h. Naturally cool to room temperature to obtain a hollow ceramic membrane.
[0047] The porosity of the hollow ceramic membrane is 28.5%. Example
[0048] The preparation method of hollow ceramic membrane is as follows:
[0049] S1: Yttrium-doped zirconium oxide powder, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone are mixed and stirred for 24 hours to obtain a spinning solution; wherein the yttrium-doped zirconium oxide powder D50=0.80μm; the mass ratio of the yttrium-doped zirconium oxide, polyethersulfone, N, N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0;
[0050] S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05 MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 20 ml / min. After passing through an air gap of 1.5 cm, the two enter the water and gel into a hollow fiber membrane. Among them, the diameters of the inner tube and outer tube of the nozzle in the electrostatic equipment are 2.5 mm and 1.0 mm respectively.
[0051] S3: drying the solidified hollow fiber membrane at room temperature for 24 h;
[0052] S4: Raise the temperature to 700°C at a rate of 2°C / min and keep it at that temperature for 2 h, then raise the temperature to 1320°C at a rate of 5°C / min and keep it at that temperature for 5 h. Naturally cool to room temperature to obtain a hollow ceramic membrane.
[0053] The porosity of the hollow ceramic membrane is 22.9%. Example
[0054] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0055] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace for homogenization treatment at a temperature of 440° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0056] Si is 0.2%;
[0057] Mg: 0.5%;
[0058] Zn: 0.25%;
[0059] Ce: 0.2%
[0060] The balance is Al;
[0061] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0062] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0063] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0064] Si is 0.2%;
[0065] Mg: 0.5%;
[0066] Zn: 0.25%;
[0067] Ce: 0.2%
[0068] The balance is Al;
[0069] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0070] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0071] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 450° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0072] Si is 0.2%;
[0073] Mg: 0.5%;
[0074] Zn: 0.25%;
[0075] Ce: 0.2%
[0076] The balance is Al;
[0077] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0078] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0079] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 25 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0080] Si is 0.2%;
[0081] Mg: 0.5%;
[0082] Zn: 0.25%;
[0083] Ce: 0.2%
[0084] The balance is Al;
[0085] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0086] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0087] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 30 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0088] Si is 0.2%;
[0089] Mg: 0.5%;
[0090] Zn: 0.25%;
[0091] Ce: 0.2%
[0092] The balance is Al;
[0093] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0094] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0095] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 5wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0096] Si is 0.2%;
[0097] Mg: 0.5%;
[0098] Zn: 0.25%;
[0099] Ce: 0.2%
[0100] The balance is Al;
[0101] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0102] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0103] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 7wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0104] Si is 0.2%;
[0105] Mg: 0.5%;
[0106] Zn: 0.25%;
[0107] Ce: 0.2%
[0108] The balance is Al;
[0109] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0110] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0111] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 10wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0112] Si is 0.2%;
[0113] Mg: 0.5%;
[0114] Zn: 0.25%;
[0115] Ce: 0.2%
[0116] The balance is Al;
[0117] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0118] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0119] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0120] Si is 0.2%;
[0121] Mg: 0.5%;
[0122] Zn: 0.25%;
[0123] Ce: 0.2%
[0124] The balance is Al;
[0125] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, with the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy being 1:3, and cool naturally in the air. Example
[0126] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0127] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0128] Si is 0.2%;
[0129] Mg: 0.5%;
[0130] Zn: 0.25%;
[0131] Ce: 0.2%
[0132] The balance is Al;
[0133] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, with the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy being 1:5, and cool naturally in the air. Example
[0134] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0135] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0136] Si is 0.4%;
[0137] Mg: 0.8%;
[0138] Zn: 0.3%;
[0139] Ce: 0.25%
[0140] The balance is Al;
[0141] Step 2: Place the hollow ceramic membrane prepared in Example 1 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0142] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0143] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0144] Si is 1.0%;
[0145] Mg: 1.5%;
[0146] Zn: 0.5%;
[0147] Ce: 0.35%
[0148] The balance is Al;
[0149] Step 2: Place the hollow ceramic membrane prepared in Example 3 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air. Example
[0150] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0151] Step 1: placing an aluminum alloy substrate and titanium diboride particles with a particle size of 1-20 μm into a heat treatment furnace and homogenizing them at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0152] Si is 0.6%;
[0153] Mg: 1.0%;
[0154] Zn: 0.4%;
[0155] Ce: 0.3%
[0156] The balance is Al;
[0157] Step 2: Place the hollow ceramic membrane prepared in Example 4 in a vehicle body panel mold, pour the reinforced aluminum alloy into the mold, the volume ratio of the hollow ceramic membrane to the reinforced aluminum alloy is 1:4, and cool naturally in the air.
[0158] The difference between this comparative example and Example 6 is that it does not contain reinforcing particles, specifically:
[0159] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0160] Step 1: placing an aluminum alloy substrate in a heat treatment furnace and subjecting it to a heat treatment at 445° C. for 28 hours to obtain an aluminum alloy; the aluminum alloy substrate comprises the following components:
[0161] Si is 0.2%;
[0162] Mg: 0.5%;
[0163] Zn: 0.25%;
[0164] Ce: 0.2%
[0165] The balance is Al;
[0166] Step 2: Place the hollow ceramic membrane prepared in Example 2 in a vehicle body panel mold, pour aluminum alloy into the mold with a volume ratio of the hollow ceramic membrane to the aluminum alloy being 1:4, and cool naturally in the air.
[0167] The difference between this comparative example and Example 6 is that the hollow ceramic membrane is not woven, specifically:
[0168] A method for preparing a high-stamping automobile aluminum alloy body plate material, the preparation steps are as follows:
[0169] Step 1: placing an aluminum alloy substrate and titanium diboride particles prepared in Example 2 with a particle size of 1-20 μm into a heat treatment furnace for homogenization treatment at a temperature of 445° C. for 28 hours to obtain a reinforced aluminum alloy; wherein the addition amount of titanium diboride particles is 9wt.% of the aluminum alloy; and the aluminum alloy substrate comprises the following components:
[0170] Si is 0.2%;
[0171] Mg: 0.5%;
[0172] Zn: 0.25%;
[0173] Ce: 0.2%
[0174] The balance is Al;
[0175] Step 2: Pour the reinforced aluminum alloy into the mold and cool it naturally in the air.
[0176] The thickness of the body panel material of each embodiment is 1 mm.
[0177] The hardening index n is determined according to the national standard GB / T 5028-2008. The higher the hardening index, the better the stamping performance.
[0178] Mechanical properties test: The equipment used for tensile mechanical properties test is Z100 universal material testing machine, and the tensile rate is 5×10 -4 m / s, tensile sample gauge length 10 mm, 3 sets of data were measured for each sample and the average value was taken.
[0179] Table 1 Characterization of mechanical properties of aluminum alloy materials in various examples
[0180] Hardening index n Tensile strength (MPa) Yield strength (MPa) Elongation (%) Example 5 0.38 58.3 33.7 32.2 Example 6 0.40 59.1 33.9 34.7 Example 7 0.39 59.4 34.1 34.0 Example 8 0.37 58.1 33.5 33.9 Example 9 0.39 59.0 33.8 34.4 Example 10 0.35 50.9 30.2 34.1 Embodiment 11 0.36 53.4 30.8 34.4 Example 12 0.38 58.7 33.7 34.5 Embodiment 13 0.33 54.3 31.6 33.9 Embodiment 14 0.38 58.5 32.9 34.4 Embodiment 15 0.35 54.9 32.0 34.0 Example 16 0.37 57.7 32.4 34.3 Embodiment 17 0.38 58.8 33.8 34.5 Comparative Example 1 0.39 50.3 28.9 34.4 Comparative Example 2 0.29 50.0 27.8 24.1 .
Claims
1. A high stamping performance automotive aluminum alloy body panel material, It is characterized in that It is composed of a hollow ceramic membrane and a reinforced aluminum alloy. The hollow ceramic membrane is made by an electrostatic spinning method. The reinforced aluminum alloy is composed of an aluminum alloy substrate and reinforced particles. The aluminum alloy substrate is composed of the following components: Si: 0.2-1.0%; Mg: 0.5-1.5%; Zn: 0.2-0.5%; Ce is 0.2-0.35%; The balance is Al; The preparation method of the hollow ceramic membrane is as follows: S1: taking yttrium-doped zirconium oxide powder, polyethersulfone, N,N-dimethylpyrrolidone and polyvinylpyrrolidone, mixing and stirring for 24 hours to obtain a spinning solution; the mass ratio of yttrium-doped zirconium oxide, polyethersulfone, N,N-dimethylpyrrolidone and polyvinylpyrrolidone is 60.5:7.5:30.5:1.0; S2: Add the spinning solution into the spinning equipment, vacuum degassing, and the spinning solution passes through the outer tube spinneret at a pressure of 0.05MPa. The core liquid in the inner tube is 90% N-methylpyrrolidone aqueous solution. The core liquid flow rate is 15-20ml / min. After the two pass through an air gap of 1.5cm, they enter the water and gel into a hollow fiber membrane; S3: drying the solidified hollow fiber membrane at room temperature for 24 hours; S4: heating to 700°C at a rate of 2°C / min and keeping the temperature for 2h, then heating to 1320°C at a rate of 5°C / min and keeping the temperature for 5h, and naturally cooling to room temperature to obtain a hollow ceramic membrane; The reinforcing particles are titanium diboride particles, and the added amount is 5-10wt.% of the aluminum alloy substrate.
2. A high stamping performance automotive aluminum alloy body panel material according to claim 1, It is characterized in that The porosity of the hollow ceramic membrane is 20-40%.
3. The high stamping performance automotive aluminum alloy body panel material according to claim 1, It is characterized in that Yttrium-doped zirconium oxide powder D50 = 0.80 μm.
4. The high stamping performance automotive aluminum alloy body panel material according to claim 1, It is characterized in that The diameters of the inner tube and outer tube of the nozzle in the spinning equipment are 2.5 mm and 1.0 mm respectively.
5. The high stamping performance automotive aluminum alloy body panel material according to claim 1, It is characterized in that The particle size of the titanium diboride particles is 1-20 μm.
Citation Information
Patent Citations
Method for preparing multichannel ceramic hollow fiber membranes
CN103349918A
High baking varnish hardening aluminum alloy material for external car body plate and preparation method thereof
CN103757507A
Hollow fiber ceramic membrane production method
CN104785123A
Diamond / aluminum composite material decorated with ceramic membrane and non-pressure infiltration preparation technology thereof
CN110643860A
TiB2 particulate ceramic reinforced Al-alloy metal-matrix composites
CN1180383A