Electric resistance welded steel pipe and method for manufacturing the same
By controlling dislocation motion and chemical composition, the problems of high yield ratio and low toughness of resistance welded steel pipes in thick-walled materials are solved, and resistance welded steel pipes with low yield ratio and high toughness are realized, which are suitable for large structures.
Patent Information
- Application Number
- CN202180066581.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-09-15
AI Technical Summary
It is difficult for existing electric resistance welded steel pipes to maintain a low yield ratio while ensuring high toughness. Especially for thick-walled materials with a wall thickness of more than 15 mm, the yield ratio increases.
By controlling the proportion of movable dislocations, suppressing dislocation movement and allowing them to remain within the grains, and using low-temperature roll forming and resistance welding processes, we ensure that the bcc phase volume ratio of the base material is high and the average crystal grain size is small. With a specific chemical composition, the A value is controlled to be above 0.55 and below 0.85 to reduce the yield ratio and improve toughness.
This is a resistance welded steel pipe that can achieve both low yield ratio and high toughness even for thick-walled materials. It is suitable for large structures such as civil engineering structures and pipeline pipes, and has improved buckling resistance and earthquake resistance.
Smart Images

Figure CN116234644B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electric resistance welded steel pipe suitable for civil engineering and building structures, pipelines and the like, and a method for manufacturing the same. Background Art
[0002] Steel pipes used for large structures such as civil engineering structures and pipelines are required to have a low yield ratio and high toughness from the viewpoints of buckling resistance and impact resistance.
[0003] One of the steel pipes used for the above-mentioned large structures is an electric resistance welded steel pipe. The electric resistance welded steel pipe is a steel pipe manufactured by continuously unwinding a hot-rolled steel plate (hot-rolled steel strip) wound into a coil and cold rolling it to form a cylindrical open pipe, melting the butted portion of the open pipe in the pipe circumferential direction by high-frequency resistance heating, performing resistance welding by pressure-joining by upsetting with an extrusion roll, and reducing the diameter to a predetermined outer diameter by a sizing roll.
[0004] Since electric resistance welded steel pipes are continuously produced by cold working, they have advantages such as high productivity and shape accuracy, but they have the disadvantage of high yield ratio because the raw material undergoes work hardening during the pipe making process. In addition, the thicker the wall, the greater the work hardening during the pipe making process, so there is a problem that the yield ratio after pipe making becomes even higher.
[0005] As a technology for solving the above-mentioned problems, for example, electric resistance welded steel pipes are proposed in Patent Documents 1 and 2. Patent Document 1 discloses a thick-walled electric resistance welded steel pipe, wherein the metal structure of the base steel plate contains 50 to 92% of polygonal ferrite by area ratio, the average grain size of the polygonal ferrite is 15 μm or less, the hardness of the electric resistance welded portion is Hv160 to 240, and the structure of the electric resistance welded portion is bainite, fine-grained ferrite and pearlite, or fine-grained ferrite and bainite.
[0006] Patent Document 2 discloses a rolled electric resistance welded steel pipe for line pipe, wherein in the metal structure of the wall thickness center portion of the base material portion, the polygonal ferrite fraction is 60 to 90%, the average grain size is 15 μm or less, the area ratio of grains with a grain size of 20 μm or more, that is, the coarse grain ratio is 20% or less, and the yield ratio in the pipe axis direction is 80 to 95%.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent No. 5293903
[0010] Patent Document 2: Japanese Patent No. 6260757 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The electric resistance welded steel pipes described in Patent Documents 1 and 2 have grain refinement to ensure high toughness. However, if the grains are refined, the yield ratio increases, so it is difficult to achieve both a low yield ratio and high toughness for thick-walled materials with a wall thickness exceeding 15 mm.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electric resistance welded steel pipe having a low yield ratio and high toughness suitable for large structures such as civil engineering structures and pipelines, and a method for manufacturing the same.
[0014] Here, the "low yield ratio" in the present invention means that the yield ratio in the tube axis direction (=yield stress (MPa) / tensile strength (MPa)×100) is 90% or less, preferably 85% or less.
[0015] The term "high toughness" used in the present invention means that the Charpy absorbed energy of the base material at -40°C is 100 J or more, preferably 150 J or more.
[0016] It should be noted that the yield stress, tensile strength, and Charpy absorbed energy can be measured by the methods described in the examples described later.
[0017] Methods used to solve problems
[0018] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, they have found that, in the deformation of electric resistance welded steel pipes, plastic deformation occurs due to the movement of mobile dislocations at the initial stage of deformation, i.e., at a stage of relatively low stress. Specifically, it has been found that, even for electric resistance welded steel pipes with equal dislocation density, the higher the proportion of mobile dislocations, the lower the yield stress. In addition, it has been found that, by roll-forming the hot-rolled steel sheet at a low temperature, the movement of dislocations introduced into the grains is suppressed, and the dislocations are not cellularized, but remain in the grains in the form of mobile dislocations.
[0019] It was found that if mobile dislocations are controlled within an appropriate range and remain in the crystal grains, the yield ratio of the electric resistance welded steel pipe is reduced and the toughness is improved even in the case of a thick-walled material.
[0020] The present invention has been accomplished based on the above findings and includes the following gist.
[0021] [1] An electric resistance welded steel pipe having a base material portion and a weld portion, wherein:
[0022] In the steel structure of the center of the wall thickness of the above-mentioned base material part,
[0023] The volume fraction of the bcc phase is 80% or more.
[0024] The average crystal grain size is less than 15.0 μm.
[0025] The A value represented by the formula (1) is 0.55 or more and 0.85 or less.
[0026] The yield ratio in the pipe axis direction is less than 90%.
[0027] The Charpy absorbed energy of the base material portion at -40°C is 100 J or more.
[0028] A=φ / ((πρ / 2) 1 / 2 ×b)…(1)
[0029] Here, in formula (1),
[0030] φ: a parameter indicating the degree of processing obtained by X-ray diffraction,
[0031] ρ: dislocation density (m -2 ),
[0032] b: Burgers vector of dislocation (m),
[0033] π: Pi.
[0034] [2] The electric resistance welded steel pipe according to [1], wherein the base material portion has a composition comprising, by mass%, C: 0.001% to 0.30%, Si: 0.01% to 2.0%, Mn: 0.20% to 3.0%, P: 0.050% to 0.020% to 0.020%, Al: 0.005% to 0.10%, N: 0.010% to 0.15% to Ti, and the balance being Fe and inevitable impurities.
[0035] [3] The electric resistance welded steel pipe according to [2], further comprising, in addition to the above component composition, one or more selected from the group consisting of Cu: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Mo: 1.0% or less, Nb: 0.15% or less, V: 0.15% or less, Ca: 0.010% or less, and B: 0.010% or less, in terms of mass %.
[0036] [4] The electric-resistance welded steel pipe according to any one of [1] to [3], wherein the wall thickness of the base material portion is 15 mm or more and 30 mm or less.
[0037] [5] The electric-resistance welded steel pipe according to any one of [1] to [4], wherein the total volume fraction of ferrite and bainite in the steel structure of the center portion of the wall thickness of the base material portion is 85% or more.
[0038] [6] A method for producing an electric resistance welded steel pipe, which is the method for producing an electric resistance welded steel pipe according to any one of [1] to [5], comprising:
[0039] A hot rolling process of heating a steel material to a heating temperature of 1100° C. to 1300° C., and then hot rolling the steel material under the conditions of a rough rolling end temperature of 850° C. to 1150° C., a finish rolling end temperature of 750° C. to 900° C., and a total reduction ratio of 50% or more at 930° C. to obtain a hot-rolled sheet;
[0040] A cooling step of cooling the hot rolled sheet at an average cooling rate of 5°C / s to 30°C / s and a cooling stop temperature of 400°C to 650°C, based on the sheet thickness center temperature;
[0041] A step of coiling the hot-rolled sheet at a temperature of 400° C. to 650° C. to obtain a hot-rolled steel sheet;
[0042] A pipe making step of forming the hot-rolled steel sheet into a cylindrical shape at a temperature of -40°C or less by roll forming and performing electric resistance welding to obtain a steel pipe raw material; and
[0043] The steel pipe material is reduced in diameter at a temperature of -40°C or lower to obtain a sizing step of obtaining an electric resistance welded steel pipe.
[0044] [7] The method for producing an electric resistance welded steel pipe according to [6], wherein the steel material has a composition, in mass %, of C: 0.001% to 0.30%, Si: 0.01% to 2.0%, Mn: 0.20% to 3.0%, P: 0.050% to 0.020%, Al: 0.005% to 0.10%, N: 0.010% to 0.15%, and the balance is Fe and unavoidable impurities.
[0045] [8] The method for producing an electric resistance welded steel pipe according to [7], wherein, in addition to the above component composition, the steel further contains, in terms of mass %, one or more selected from the group consisting of Cu: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Mo: 1.0% or less, Nb: 0.15% or less, V: 0.15% or less, Ca: 0.010% or less, and B: 0.010% or less.
[0046] [9] The method for manufacturing an electric resistance welded steel pipe according to any one of [6] to [8], wherein the wall thickness of the base material portion of the electric resistance welded steel pipe is 15 mm or more and 30 mm or less.
[0047] Effects of the Invention
[0048] According to the present invention, it is possible to provide an electric resistance welded steel pipe having both a low yield ratio and high toughness even when the steel pipe is thick-walled, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a schematic diagram showing a pipe circumferential cross section (a cross section perpendicular to the pipe axial direction) including the periphery of a welded portion of an electric resistance welded steel pipe. DETAILED DESCRIPTION
[0050] Hereinafter, the electric resistance welded steel pipe of the present invention will be described.
[0051] The electric resistance welded steel pipe of the present invention comprises a base material portion and a weld portion (electric resistance weld portion) extending in the pipe axial direction. In the steel structure of the wall thickness center portion of the base material portion of the present invention, the volume fraction of the bcc phase is 80% or more, the average crystal grain size is 15.0 μm or less, the A value represented by the formula (1) is 0.55 or more and 0.85 or less, the yield ratio in the pipe axial direction is 90% or less, and the Charpy absorbed energy of the base material portion at -40°C is 100 J or more.
[0052] A=φ / ((πρ / 2) 1 / 2 ×b)…(1)
[0053] Here, in formula (1),
[0054] φ: a parameter indicating the degree of processing obtained by X-ray diffraction,
[0055] ρ: dislocation density (m -2 ),
[0056] b: Burgers vector of dislocation (m),
[0057] π: Pi.
[0058] First, the reasons for limiting the steel structure and properties of the electric resistance welded steel pipe of the present invention will be described.
[0059] Volume ratio of bcc phase in the center of the wall thickness of the base material: 80% or more
[0060] The bcc (body-centered cubic lattice) phase has a greater effect of temperature on the movement of dislocations than the fcc (face-centered cubic lattice) and hcp (hexagonal closest-packed structure) phases. Therefore, for the bcc phase, the effect of suppressing the movement of dislocations by lowering the temperature is greater. That is, the higher the volume fraction of the bcc phase, the more dislocation movement is suppressed when the electric resistance welded steel pipe is made at a low temperature, so that the dislocations are not easily entangled with each other, and the proportion of movable dislocations becomes higher. As a result, the yield ratio is reduced. In order to fully obtain such an effect, the volume fraction of the above-mentioned bcc phase is set to 80% or more. The volume fraction of the bcc phase is preferably 85% or more, and more preferably 90% or more.
[0061] The upper limit of the volume ratio of the bcc phase is not particularly specified. In order to obtain a bcc single-phase structure, the steel plate needs to be rapidly cooled after hot rolling, and it is difficult to completely avoid phases other than the bcc phase in the center of the wall thickness of a thick-walled material. Therefore, the bcc phase is preferably 98% or less by volume, and more preferably 97% or less by volume. The remainder other than the bcc phase is an fcc phase or cementite, and is preferably 20% or less by volume.
[0062] Here, the volume fraction of the bcc phase is measured by X-ray diffraction as described in the examples described later. After mirror polishing the cross section of the base material portion at the 90° position in the circumferential direction of the tube when the weld portion is set to 0°, which is parallel to both the tube length direction and the wall thickness direction, electrolytic polishing of 100 μm is performed to remove the surface processing layer, and a test piece is prepared in such a way that the diffraction surface is the center of the wall thickness, and the steel structure is measured using the test piece. In the measurement, the volume fraction of the bcc phase is calculated from the integrated intensity of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron using Mo Kα rays. In addition, the volume fraction of the fcc phase is also calculated at the same time.
[0063] Average grain size of the grains in the center of the wall thickness of the base material: 15.0 μm or less
[0064] In the present invention, the region surrounded by the boundary where the orientation difference of adjacent crystals is 15° or more is set as a crystal grain. When the average crystal grain size of the crystal grains in the central part of the wall thickness of the parent material portion exceeds 15.0 μm, the total area of the grain boundaries that become an obstacle to the propagation of cracks is small, so the high toughness targeted in the present invention cannot be obtained. Therefore, the above-mentioned average crystal grain size is set to less than 15.0 μm. The average crystal grain size is preferably less than 10.0 μm, more preferably less than 8.0 μm. It should be noted that the smaller the average crystal grain size, the higher the yield ratio, so the average crystal grain size is preferably more than 2.0 μm. The average crystal grain size is more preferably more than 3.0 μm.
[0065] Here, the average crystal grain size refers to the average equivalent circle diameter of the crystal grain when the region surrounded by the boundary where the orientation difference of adjacent crystals is 15° or more is set as the crystal grain (grain boundary). The equivalent circle diameter (crystal grain size) refers to the diameter of a circle having the same area as the crystal grain as the object.
[0066] The determination of the average crystal grain size can be carried out by the method described in the embodiments described later. The cross section of the base material portion at the 90° position in the circumferential direction of the tube when the weld portion is set to 0° and parallel to both the tube length direction and the wall thickness direction is mirror-polished to prepare a test piece. Using the SEM / EBSD method, a histogram of the grain size distribution in the central part of the wall thickness of the test piece is calculated (the horizontal axis is set to the grain size and the vertical axis is set to a graph of the existence ratio of each grain size), and the arithmetic mean of the grain size is obtained as the average grain size. The measurement conditions are set to acceleration voltage: 15kV, measurement area: 500μm×500μm, and measurement step length (measurement resolution): 0.5μm. It should be noted that in the analysis of the grain size, crystals with a grain size of less than 2.0μm are excluded from the analysis object as measurement noise.
[0067] A value: 0.55 or more and 0.85 or less
[0068] The A value is a parameter related to the distribution state of dislocations and can be expressed by the above formula (1).
[0069] Formula (1) shows that φ is a parameter indicating the degree of processing obtained by X-ray diffraction, ρ is the dislocation density (m -2 ), and b: the Burgers vector (m) of the dislocation (reference 3).
[0070] A larger value of A indicates a tendency that the dislocations introduced into the crystal grains are uniformly distributed, the dislocations are not cellularized, and the proportion of dislocations remaining in the crystal grains as mobile dislocations is high.
[0071] Cellularized dislocations are entangled with each other, so high stress is required to start moving. On the other hand, compared with cellularized dislocations, mobile dislocations can move at lower stress. Therefore, the more mobile dislocations there are in the grain (the higher the proportion of mobile dislocations), the lower the stress at which plastic deformation starts, and thus the yield ratio becomes lower. In addition, the more mobile dislocations there are in the grain, the more plastic deformation at the front end of the crack is promoted, so it is difficult to produce dissociative failure, resulting in higher toughness. For such reasons, it is important to satisfy the above formula (1) in the present invention.
[0072] It is known that in the existing electric resistance welded steel pipe with dislocation cellization, the A value represented by the above formula (1) is less than 0.55. Therefore, in the present invention, in order to ensure a sufficient amount of movable dislocations required to obtain the desired yield ratio, the A value is set to 0.55 or more. The larger the A value, the more preferred, but in order to make the A value larger, it is necessary to make the pipe at a lower temperature. Therefore, from the perspective of the increase in pipe making load due to the increase in deformation resistance, temperature management of hydraulic devices, etc., and cooling costs, the A value is set to 0.85 or less. The A value is preferably 0.60 or more, and preferably 0.80 or less. The A value is more preferably 0.61 or more, and more preferably 0.78 or less.
[0073] It should be noted that the A value can be controlled within the above range by controlling the production conditions (the temperature of the pipe making process and the diameter reducing process) described later.
[0074] Here, the "dislocation density ρ", "parameter φ" and "Burgers vector b" in the above formula (1) can be obtained by the method described in the examples described later.
[0075] Regarding the dislocation density ρ, after mirror polishing the cross-section of the base material portion parallel to both the tube length direction and the wall thickness direction, electrolytic polishing of 100 μm was performed to remove the surface processing layer, and a test piece was made in such a way that the diffraction surface was the central part of the wall thickness, and the test piece was used for X-ray diffraction. Based on the results, the dislocation density ρ can be calculated using the modified Williamson-Hall method and the modified Warren-Averbach method (references 1 and 2). The parameter φ can be calculated based on the above X-ray diffraction results using the direct fitting (direct-fitting) / modified Williamson-Hall method (reference 3). The Burgers vector b is the interatomic distance of <111>, which is the slip direction of bcc iron, and can be calculated using 0.248×10 -9 m.
[0076] Reference 1: T. Ungar and A. Borbely: Appl. Phys. Lett., 69 (1996), 3173.
[0077] Reference 2: M. Kumagai, M. Imafuku, S. Ohya: ISIJ International, 54 (2014), 206.
[0078] Reference 3: S. Takaki, T. Masumura and T. Tsuchiyama: ISIJ International, 59 (2019), 567.
[0079] Yield ratio in the tube axis direction: less than 90%
[0080] The yield ratio (=yield stress (MPa) / tensile strength (MPa)×100) of the parent material portion at the 90° position in the circumferential direction of the pipe of the electric resistance welded steel pipe of the present invention when the weld portion is set to 0° in the pipe axial direction is 90% or less. When the yield ratio exceeds 90%, the seismic resistance when used for columns of civil engineering structures, etc., and the seismic resistance and buckling resistance when used for pipelines are reduced. The above-mentioned yield ratio is preferably 87% or less, and more preferably 86% or less. From the viewpoint of ensuring the necessary yield strength, the above-mentioned yield ratio is preferably 55% or more, more preferably 65% or more, and further preferably 75% or more.
[0081] Charpy absorbed energy of base material at -40℃: 100J or more
[0082] The Charpy absorbed energy of the base material of the electric resistance welded steel pipe of the present invention at -40°C is 100 J or more. If it is less than 100 J, the seismic resistance is reduced when used for columns of civil engineering structures and pipelines. The above Charpy absorbed energy is preferably 150 J or more, and more preferably 160 J or more. In addition, when the Charpy absorbed energy is high, the average crystal grain size is small and the yield ratio becomes high, so it is preferably 500 J or less, and more preferably 400 J or less.
[0083] Here, as described in the examples below, the yield strength, tensile strength, and yield ratio can be obtained by performing a tensile test in accordance with the provisions of JIS Z 2241. As described in the examples below, the Charpy absorbed energy can be obtained by performing a Charpy impact test at a test temperature of -40°C using a V-notch standard test piece in accordance with the provisions of JIS Z 2242.
[0084] The electric resistance welded steel pipe of the present invention has the above-mentioned steel structure to obtain the above-mentioned properties. For the purpose of further improving the properties, the steel structure of the present invention may also have the following constitution.
[0085] In the steel structure of the center of the wall thickness of the parent material part, the total volume ratio of ferrite and bainite is preferably 85% or more relative to the entire steel structure of the center of the wall thickness of the parent material part. The remaining structure other than ferrite and bainite includes one or more selected from pearlite, martensite, and austenite. The total volume ratio of the remaining structure is preferably 15% or less.
[0086] Ferrite is a bcc phase and is a soft structure. Bainite is a bcc phase, which is harder than ferrite, softer than pearlite, martensite and austenite, and is a structure with excellent toughness. When hard structures are mixed in ferrite and bainite, the yield ratio decreases. On the other hand, due to stress concentration caused by the hardness difference, the interface easily becomes the starting point of fracture, resulting in reduced toughness. Therefore, the total volume ratio of ferrite and bainite is preferably 85% or more. More preferably, it is 90% or more. In addition, it is preferably 98% or less, and more preferably 97% or less.
[0087] Pearlite and martensite are a mixed structure of bcc phase and cementite and bcc phase, respectively, and both are hard structures. It should be noted that, here, pearlite is approximately treated as a bcc phase. Pearlite is a structure that reduces the yield ratio by mixing with a soft structure, but on the other hand, it is a structure that reduces toughness, and is preferably set to 15% or less, preferably set to 0% or more. Pearlite is more preferably set to 13% or less, and more preferably set to 1% or more.
[0088] Martensite is a structure that reduces the yield ratio by mixing with the soft structure, but reduces toughness, and is preferably set to 15% or less, preferably 0% or more. Martensite is more preferably set to 13% or less, and more preferably 1% or more.
[0089] Austenite is an fcc phase and is a hard structure. Austenite is a structure that reduces the yield ratio by mixing with a soft structure, but on the other hand, it is a structure that reduces toughness, and is preferably set to 10% or less, preferably set to 0% or more. Austenite is more preferably set to 8% or less, and more preferably set to 1% or more.
[0090] The above-mentioned various structures except austenite use the austenite grain boundary or the deformation band in the austenite grain as the nucleation site. In hot rolling, by increasing the reduction at a low temperature where the recrystallization of austenite is not easy to occur, a large number of dislocations can be introduced into austenite to make the austenite finer, and a large number of deformation bands can be introduced into the grains. As a result, the area of the nucleation site increases and the nucleation frequency increases, which can make the steel structure finer.
[0091] In the present invention, even if the above-mentioned steel structure exists within the range of ±1.0 mm in the wall thickness direction with the wall thickness center of the parent material part as the center, the above-mentioned effect can be obtained in the same manner. Therefore, in the present invention, "the steel structure in the wall thickness center of the parent material part" means that the above-mentioned steel structure exists at any place within the range of ±1.0 mm in the wall thickness direction with the wall thickness center as the center.
[0092] Here, the observation of the steel structure can be carried out by the method described in the embodiments described later. First, the observation surface is cut in a manner that the cross section of the parent material part at the 90° position in the circumferential direction of the tube is perpendicular to the length direction of the tube and becomes the central part of the wall thickness, and after grinding, it is corroded using a nitric acid alcohol solution to make a test piece for tissue observation. In the tissue observation, an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) is used to observe and photograph the structure of the central part of the wall thickness. Then, based on the obtained optical microscope image and SEM image, the area ratio of bainite and the remainder (ferrite, pearlite, martensite, austenite) is calculated. The area ratio of each organization is observed in more than 5 fields of view and calculated as the average value of the values obtained in each field of view. It should be noted that in the present invention, the area ratio obtained by tissue observation is used as the volume ratio of each organization.
[0093] Ferrite is a product of diffusion phase transformation, showing a low dislocation density and basically restored structure. Polygonal ferrite and near-polygonal ferrite are also included in ferrite.
[0094] Bainite is a duplex structure of lath-shaped ferrite and cementite with high dislocation density.
[0095] Pearlite is a eutectic structure of iron and iron carbide (ferrite + cementite), and appears as a layered structure with linear ferrite and cementite arranged alternately.
[0096] Martensite is a bcc phase, a lath-shaped low-temperature transformation structure with a very high dislocation density. In SEM images, it shows a bright contrast compared to ferrite and bainite.
[0097] It should be noted that martensite and austenite are difficult to identify in optical microscope images and SEM images, so the area ratio of the structure observed in the form of martensite or austenite is measured based on the obtained SEM image, and the value obtained by subtracting the volume ratio of austenite measured by the method described later from the measured value is used as the volume ratio of martensite.
[0098] The volume fraction of austenite was measured by X-ray diffraction using a test piece prepared by the same method as the test piece used for the measurement of dislocation density. The volume fraction of austenite was obtained from the integrated intensity of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron.
[0099] Next, from the viewpoint of ensuring the above-mentioned characteristics and steel structure, etc., the preferred range of the component composition in the electric resistance welded steel pipe of the present invention and the reasons for the limitation are described.
[0100] The reasons for limiting the chemical composition of the base material portion of the electric resistance welded steel pipe will be described. It should be noted that, in this specification, "%" indicating the steel composition means "mass %" unless otherwise specified.
[0101] The base material part of the present invention preferably has a composition containing, in mass%, C: 0.001% to 0.30%, Si: 0.01% to 2.0%, Mn: 0.20% to 3.0%, P: 0.050% to 0.020%, Al: 0.005% to 0.10%, N: 0.010% to 0.15% and Ti: 0.15% to 0.15%, with the balance being Fe and unavoidable impurities.
[0102] C: 0.001% or more and 0.30% or less
[0103] C is an element that increases the strength of steel by solid solution strengthening. In addition, C is an element that contributes to the refinement of the structure by lowering the starting temperature of ferrite transformation. In order to obtain such an effect, it is necessary to contain more than 0.001% C. In addition, C promotes the formation of pearlite, improves hardenability and contributes to the formation of martensite and the stabilization of austenite, and is therefore also an element that contributes to the formation of hard phases. When the C content exceeds 0.30%, the proportion of hard phases increases, the toughness decreases, and the weldability also deteriorates. Therefore, the C content is set to be greater than 0.001% and less than 0.30%. The C content is preferably greater than 0.010%, and more preferably greater than 0.040%. In addition, the C content is preferably less than 0.27%, and more preferably less than 0.25%.
[0104] Si: 0.01% or more and 2.0% or less
[0105] Si is an element that increases the strength of steel by solid solution strengthening. In order to obtain such an effect, 0.01% or more of Si is contained. However, when the Si content exceeds 2.0%, the yield ratio becomes higher and the toughness decreases. Therefore, the Si content is set to be greater than 0.01% and less than 2.0%. The Si content is preferably greater than 0.05%, more preferably greater than 0.10%. In addition, the Si content is preferably less than 1.0%, more preferably less than 0.50%.
[0106] Mn: 0.20% or more and 3.0% or less
[0107] Mn is an element that increases the strength of steel by solid solution strengthening. In addition, Mn is an element that contributes to the refinement of the steel structure by lowering the ferrite transformation start temperature. In order to obtain such an effect, it is necessary to contain more than 0.20% Mn. However, when the Mn content exceeds 3.0%, the yield stress becomes high due to solid solution strengthening and the refinement of the steel structure, and the yield ratio targeted in the present invention cannot be obtained. Therefore, the Mn content is set to be greater than 0.20% and less than 3.0%. The Mn content is preferably greater than 0.40%, and more preferably greater than 0.60%. In addition, the Mn content is preferably less than 2.5%, and more preferably less than 2.0%.
[0108] P: 0.050% or less
[0109] P segregates at grain boundaries, causing uneven materials, so it is preferred to reduce it as much as possible as an unavoidable impurity, but it can be allowed to be up to 0.050%. Therefore, the P content is set to 0.050% or less. The P content is preferably 0.020% or less, and more preferably 0.010% or less. It should be noted that the lower limit of the P content is not specifically specified, but excessive reduction leads to a rise in smelting costs, so the P content is preferably set to 0.002% or more.
[0110] S: 0.020% or less
[0111] S usually exists in the form of MnS in steel, but MnS is stretched thinner during the hot rolling process, which has an adverse effect on ductility. Therefore, in the present invention, it is preferred to reduce S as much as possible, but it can be allowed to be up to 0.020%. Therefore, the S content is set to less than 0.020%. The S content is preferably less than 0.010%, and more preferably less than 0.008%. It should be noted that the lower limit of the S content is not particularly specified, but excessive reduction leads to a rise in smelting costs, so the S content is preferably set to more than 0.0002%.
[0112] Al: 0.005% or more and 0.10% or less
[0113] Al is an element that acts as a strong deoxidizer. In order to obtain such an effect, it is necessary to contain more than 0.005% Al. However, when the Al content exceeds 0.10%, weldability deteriorates, and the number of alumina inclusions increases, and the surface properties deteriorate. In addition, the toughness of the weld is also reduced. Therefore, the Al content is set to be greater than 0.005% and less than 0.10%. The Al content is preferably greater than 0.010%, and more preferably greater than 0.015%. The Al content is preferably less than 0.080%, and more preferably less than 0.070%.
[0114] N: 0.010% or less
[0115] N is an inevitable impurity and an element that has the effect of firmly fixing the movement of dislocations and thus reducing toughness. In the present invention, N is preferably reduced as an impurity as much as possible, but the N content can be allowed to be up to 0.010%. Therefore, the N content is set to 0.010% or less. The N content is preferably 0.0080% or less. From the viewpoint of refining cost, the N content is preferably 0.0008% or more, and more preferably 0.0010% or more.
[0116] Ti: 0.15% or less
[0117] Ti is an element that forms fine carbides and nitrides in steel and helps to improve the strength of steel. In addition, since Ti has a high affinity with N, it is an element that converts N in steel into nitrides and makes it harmless, and also helps to improve the toughness of steel. In order to obtain the above-mentioned effects, it is preferred to contain 0.001% or more of Ti. However, when the Ti content exceeds 0.15%, the yield ratio becomes higher and the toughness decreases. Therefore, the Ti content is set to 0.15% or less. The Ti content is more preferably 0.005% or more, and further preferably 0.008% or more. The Ti content is more preferably 0.13% or less, and further preferably 0.10% or less.
[0118] The balance other than the above components is Fe and inevitable impurities. However, as an inevitable impurity, 0.0050% or less of O may be contained. Here, O refers to all oxygen including O in the form of oxides.
[0119] In the present invention, it is preferred to use the above components as the basic component composition. In the present invention, in order to further improve the characteristics, on the basis of the above basic components, one or more selected from Cu: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Mo: 1.0% or less, Nb: 0.15% or less, V: 0.15% or less, Ca: 0.010% or less, B: 0.010% or less may be contained as needed.
[0120] Cu: 1.0% or less (including 0%)
[0121] Cu is an element that increases the strength of steel by solid solution strengthening, and can be contained as needed. In order to obtain the above-mentioned effect, when Cu is contained, the Cu content is preferably set to 0.01% or more. On the other hand, when more than 1.0% Cu is contained, it is possible to cause a decrease in toughness and deterioration in weldability. Therefore, when Cu is contained, the Cu content is preferably set to 1.0% or less. The Cu content is more preferably 0.05% or more, and further preferably 0.10% or more. In addition, the Cu content is more preferably 0.70% or less, and further preferably 0.50% or less.
[0122] Ni: 1.0% or less (including 0%)
[0123] Ni is an element that increases the strength of steel by solid solution strengthening, and can be contained as needed. In order to obtain the above-mentioned effect, when Ni is contained, the Ni content is preferably set to 0.01% or more. On the other hand, when more than 1.0% Ni is contained, it is possible to cause a decrease in toughness and deterioration in weldability. Therefore, when Ni is contained, the Ni content is preferably set to 1.0% or less. The Ni content is more preferably 0.05% or more, and further preferably 0.10% or more. In addition, the Ni content is more preferably 0.70% or less, and further preferably 0.50% or less.
[0124] Cr: 1.0% or less (including 0%)
[0125] Cr is an element that improves the hardenability of steel and increases the strength of steel, and can be contained as needed. In order to obtain the above-mentioned effect, when Cr is contained, the Cr content is preferably set to 0.01% or more. On the other hand, when more than 1.0% Cr is contained, it is possible to cause a decrease in toughness and deterioration in weldability. Therefore, when Cr is contained, the Cr content is preferably set to 1.0% or less. The Cr content is more preferably 0.05% or more, and further preferably 0.10% or more. In addition, the Cr content is more preferably 0.70% or less, and further preferably 0.50% or less.
[0126] Mo: 1.0% or less (including 0%)
[0127] Mo is an element that improves the hardenability of steel and increases the strength of steel, and can be contained as needed. In order to obtain the above-mentioned effect, when Mo is contained, the Mo content is preferably set to 0.01% or more. On the other hand, when more than 1.0% of Mo is contained, it is possible to cause a decrease in toughness and deterioration in weldability. Therefore, when Mo is contained, the Mo content is preferably set to 1.0% or less. The Mo content is more preferably 0.05% or more, and further preferably 0.10% or more. In addition, the Mo content is more preferably 0.70% or less, and further preferably 0.50% or less.
[0128] Nb: 0.15% or less (including 0%)
[0129] Nb is an element that helps to improve the strength of steel by forming fine carbides and nitrides in steel, and also helps to refine the structure by inhibiting the coarsening of austenite during hot rolling. It can be contained as needed. In order to obtain the above-mentioned effect, when Nb is contained, it is preferred to contain 0.002% or more of Nb. However, when the Nb content exceeds 0.15%, the yield ratio becomes higher and the toughness decreases. Therefore, when Nb is contained, the Nb content is preferably set to 0.15% or less. The Nb content is more preferably 0.005% or more, and more preferably 0.010% or more. The Nb content is more preferably 0.13% or less, and more preferably 0.10% or less.
[0130] V: 0.15% or less (including 0%)
[0131] V is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in steel, and can be contained as needed. In order to obtain the above-mentioned effect, when V is contained, it is preferred to contain 0.002% or more of V. However, when the V content exceeds 0.15%, the yield ratio becomes higher and the toughness decreases. Therefore, when V is contained, the V content is preferably set to 0.15% or less. The V content is more preferably 0.005% or more, and further preferably 0.010% or more. The V content is more preferably 0.13% or less, and further preferably 0.10% or less.
[0132] Ca: 0.010% or less (including 0%)
[0133] Ca is an element that helps improve the toughness of steel by spheroidizing sulfides such as MnS that are stretched thinner in the hot rolling process, and can be contained as needed. In order to obtain the above-mentioned effect, when Ca is contained, it is preferred to contain 0.0005% or more of Ca. However, when the Ca content exceeds 0.010%, Ca oxide clusters are formed in the steel, and the toughness deteriorates. Therefore, when Ca is contained, the Ca content is preferably set to 0.010% or less. The Ca content is more preferably 0.0008% or more, and further preferably 0.0010% or more. In addition, the Ca content is more preferably 0.008% or less, and further preferably 0.0060% or less.
[0134] B: 0.010% or less (including 0%)
[0135] B is an element that contributes to the refinement of the structure by lowering the ferrite transformation start temperature, and can be contained as needed. In order to obtain the above-mentioned effect, when B is contained, it is preferred to contain 0.0003% or more of B. However, when the B content exceeds 0.010%, the yield ratio increases and the toughness deteriorates. Therefore, when B is contained, the B content is set to 0.010% or less. The B content is more preferably 0.0005% or more, and further preferably 0.0008% or more. The B content is more preferably 0.0050% or less, further preferably 0.0030% or less, and further preferably 0.0020% or less.
[0136] It should be noted that, in particular, from the viewpoint of being suitable for large structures such as civil engineering structures and pipelines, the electric resistance welded steel pipe of the present invention preferably has a wall thickness of the base material portion of 15 mm or more and 30 mm or less. From the viewpoint of low yield ratio and high toughness, it is more preferably 15 mm or more and 25 mm or less. As described above, according to the present invention, even thick-walled materials with a wall thickness exceeding 15 mm can have both low yield ratio and high toughness. As a result, when the electric resistance welded steel pipe of the present invention is used in large structures, excellent buckling resistance is exerted. In addition, for the same reason, the electric resistance welded steel pipe of the present invention preferably has an outer diameter of 350 mm or more and 750 mm or less. From the viewpoint of low yield ratio and high toughness, it is more preferably 400 mm or more and 750 mm or less.
[0137] Next, one embodiment of the method for producing an electric resistance welded steel pipe according to the present invention will be described.
[0138] In the present invention, a steel material having the above-mentioned composition is heated to a heating temperature of 1100° C. to 1300° C., and then hot-rolled under the conditions that the rough rolling end temperature is 850° C. to 1150° C., the finish rolling end temperature is 750° C. to 900° C., and the total reduction ratio at 930° C. or less is 50% or more to produce a hot-rolled sheet (hot rolling process), and then the steel material is cooled at an average cooling rate of 5° C. / s to 30° C. / s and a cooling stop temperature of 100° C. to 150° C. The hot rolled plate is cooled at a temperature of 400°C to 650°C (cooling process), and then the cooled hot rolled plate is coiled at a temperature of 400°C to 650°C to form a hot rolled steel plate (coiling process), and then the hot rolled steel plate is formed into a cylindrical shape by roll forming at a temperature of -40°C or less and resistance welded to form a steel pipe material (pipe making process), and then the steel pipe material is reduced in diameter at a temperature of -40°C or less (sizing process) to manufacture an electric resistance welded steel pipe.
[0139] It should be noted that, in the following description of the manufacturing method, unless otherwise specified, the temperature "°C" refers to the surface temperature of the steel raw material, steel plate (hot-rolled plate), and steel pipe raw material. These surface temperatures can be measured using a radiation thermometer or the like. Regarding the temperature at the center of the steel plate thickness, the temperature distribution in the cross section of the steel plate can be calculated by heat transfer analysis, and the result can be corrected by the surface temperature of the steel plate to obtain the temperature at the center of the steel plate thickness. "Hot-rolled steel plate" also includes hot-rolled plate and hot-rolled steel strip.
[0140] In the present invention, the smelting method of the steel raw material (steel billet) is not particularly limited, and any of the known smelting methods such as converter, electric furnace, vacuum melting furnace, etc. is suitable. The casting method is also not particularly limited, and the desired size can be manufactured by a known casting method such as continuous casting. It should be noted that there is no problem in applying the ingot casting-opening billet rolling method instead of the continuous casting method. The molten steel can also be further subjected to secondary refining such as ladle refining.
[0141] [Hot rolling process]
[0142] Heating temperature: 1100°C or higher and 1300°C or lower
[0143] When the heating temperature is lower than 1100°C, the deformation resistance of the rolled material becomes large and rolling becomes difficult. On the other hand, when the heating temperature exceeds 1300°C, the austenite grains coarsen, and fine austenite grains cannot be obtained in the subsequent rolling (rough rolling, finish rolling), and it is difficult to ensure the average grain size of the steel structure of the electric resistance welded steel pipe as the target in the present invention. Therefore, the heating temperature in the hot rolling process is set to be higher than 1100°C and lower than 1300°C. The heating temperature is more preferably higher than 1120°C. In addition, the heating temperature is more preferably lower than 1280°C.
[0144] It should be noted that in the present invention, after the steel billet (slab) is manufactured, it is temporarily cooled to room temperature and then heated again. In addition to such existing methods, an energy-saving direct rolling process can be applied without any problem, in which the steel billet is loaded into a heating furnace in a hot sheet state without cooling to room temperature or is rolled immediately after being slightly kept warm.
[0145] Rough rolling end temperature: 850℃ or higher and 1150℃ or lower
[0146] When the rough rolling end temperature is lower than 850°C, the surface temperature of the steel plate becomes below the ferrite transformation start temperature in the subsequent finish rolling, a large amount of processed ferrite is generated, and the yield ratio increases. On the other hand, when the rough rolling end temperature exceeds 1150°C, the reduction amount in the austenite non-recrystallization temperature range is insufficient, and fine austenite grains cannot be obtained. As a result, it is difficult to ensure the average grain size of the steel structure of the electric resistance welded steel pipe as the target in the present invention, and the toughness is reduced. The rough rolling end temperature is more preferably 860°C or higher. In addition, the rough rolling end temperature is more preferably 1000°C or lower.
[0147] Finish rolling starting temperature (preferred conditions)
[0148] The start temperature of the finishing rolling is preferably above 800°C and below 950°C. When the start temperature of the finishing rolling is lower than 800°C, the surface temperature of the steel plate becomes below the start temperature of the ferrite transformation during the finishing rolling, a large amount of processed ferrite is generated, and the yield ratio increases. On the other hand, when the start temperature of the finishing rolling exceeds 950°C, the austenite coarsens, and sufficient deformation bands are not introduced into the austenite. Therefore, it is difficult to ensure the average grain size of the steel structure targeted in the present invention, and the toughness decreases. The start temperature of the finishing rolling is more preferably above 820°C. In addition, the start temperature of the finishing rolling is preferably below 930°C.
[0149] Finish rolling end temperature: 750℃ or higher and 900℃ or lower
[0150] When the finishing temperature of the finishing rolling is lower than 750°C, the surface temperature of the steel plate becomes lower than the ferrite transformation start temperature during the finishing rolling, a large amount of processed ferrite is generated, and the yield ratio increases. On the other hand, when the finishing temperature of the finishing rolling exceeds 900°C, the reduction amount in the austenite non-recrystallization temperature range is insufficient, and fine austenite grains cannot be obtained. As a result, it is difficult to ensure the average crystal grain size of the steel structure of the electric resistance welded steel pipe as the target in the present invention, and the toughness decreases. The finishing temperature of the finishing rolling is more preferably 770°C or higher. In addition, the finishing temperature of the finishing rolling is more preferably 880°C or lower.
[0151] Total reduction ratio at 930℃ or below: 50% or more
[0152] In the present invention, by refining the subgrains in austenite in the hot rolling process, the ferrite, bainite and the remaining structure generated in the subsequent cooling process and coiling process are refined, and the steel structure of the electric resistance welded steel pipe having the strength and toughness targeted by the present invention can be obtained. In order to refine the subgrains in austenite in the hot rolling process, it is necessary to increase the reduction rate in the austenite non-recrystallization temperature range and introduce sufficient processing strain. In order to achieve the above purpose, in the present invention, the total reduction rate at 930°C or below is set to 50% or more.
[0153] When the total reduction rate at 930°C or less is less than 50%, sufficient processing strain cannot be introduced in the hot rolling process, so the structure with the average grain size targeted in the present invention cannot be obtained. The total reduction rate at 930°C or less is more preferably 55% or more, and more preferably 57% or more. There is no particular upper limit to the total reduction rate. When it exceeds 80%, the effect of improving toughness with an increase in the reduction rate becomes smaller, and only the equipment load increases. Therefore, the total reduction rate at 930°C or less is preferably 80% or less. More preferably, it is 70% or less.
[0154] The above-mentioned total reduction ratio at 930°C or lower refers to the total reduction ratio of each rolling pass in the temperature range of 930°C or lower.
[0155] [Cooling process]
[0156] After the hot rolling step, the hot rolled sheet is cooled in a cooling step. In the cooling step, the hot rolled sheet is cooled at an average cooling rate of 5°C / sec to a cooling stop temperature of 30°C / sec and a cooling stop temperature of 400°C to 650°C.
[0157] Average cooling rate from the start of cooling to the stop of cooling (end of cooling): 5°C / sec or more and 30°C / sec or less
[0158] When the average cooling rate in the temperature range from the start of cooling to the stop of cooling described later is less than 5°C / second, the nucleation frequency of ferrite or bainite is reduced, and ferrite or bainite is coarsened, so that the structure with the average grain size targeted in the present invention cannot be obtained. On the other hand, when the average cooling rate exceeds 30°C / second, a large amount of martensite is generated, and the toughness is reduced. The average cooling rate is preferably 10°C / second or more. In addition, the average cooling rate is preferably 25°C / second or less.
[0159] In addition, in the present invention, from the viewpoint of suppressing the formation of ferrite on the surface of the steel sheet before cooling, it is preferred to start cooling immediately after the finish rolling is completed.
[0160] Cooling stop temperature: 400°C or higher and 650°C or lower
[0161] When the cooling stop temperature is lower than 400°C, a large amount of martensite is generated and the toughness is reduced, based on the plate thickness center temperature of the hot-rolled plate. On the other hand, when the cooling stop temperature exceeds 650°C, the nucleation frequency of ferrite or bainite is reduced, and the ferrite or bainite is coarsened, so that the structure with the average grain size targeted in the present invention cannot be obtained. In addition, the enrichment of C into the untransformed austenite is easy to proceed, so sometimes the austenite fraction becomes high and the volume rate of the bcc phase is reduced. The cooling stop temperature is preferably above 430°C. In addition, the cooling stop temperature is preferably below 620°C.
[0162] It should be noted that, in the present invention, unless otherwise specified, the average cooling rate is set to a value (cooling rate) obtained by ((plate thickness center temperature of the hot-rolled plate before cooling - plate thickness center temperature of the hot-rolled plate after cooling) / cooling time). The cooling method may include water cooling such as spraying water from a nozzle, cooling by spraying cooling gas, etc. In the present invention, it is preferred that both sides of the hot-rolled plate are cooled under the same conditions to perform cooling operation (treatment) on both sides of the hot-rolled plate.
[0163] [Coiling process]
[0164] Coiling temperature: 400°C or higher and 650°C or lower
[0165] After the cooling process, the hot-rolled steel sheet is coiled into a coiled material by a coiling process and then cooled. In the coiling process, from the perspective of the steel sheet structure, the coiling is performed under the condition that the coiling temperature is above 400°C and below 650°C. When the coiling temperature is lower than 400°C, a large amount of martensite is generated and the toughness is reduced. When the coiling temperature exceeds 650°C, the nucleation frequency of ferrite or bainite is reduced, and the ferrite or bainite is coarsened, so that the structure with the average grain size targeted in the present invention cannot be obtained. In addition, the enrichment of C into the untransformed austenite is easy to proceed, so sometimes the austenite fraction becomes high and the volume fraction of the bcc phase decreases. The coiling temperature is preferably above 430°C. In addition, the coiling temperature is preferably below 620°C.
[0166] [Pipe making process]
[0167] Temperature of hot rolled steel plate: below -40℃
[0168] After the coiling process, the pipe making process is carried out. In the pipe making process, the hot-rolled steel sheet is continuously unwound and formed into a cylindrical open pipe (round steel pipe) by roll forming at a temperature below -40°C. The circumferential butt joint of the open pipe is melted by high-frequency resistance heating, and at the same time, the steel pipe raw material is made by resistance welding by pressure-joining by upsetting with an extrusion roll.
[0169] As a method for cooling the hot-rolled steel sheet in the pipe manufacturing process, the hot-rolled steel sheet wound into a coil is cooled in advance to -40°C or less. Alternatively, a part of the pipe manufacturing equipment may be cooled to -40°C or less.
[0170] By setting the temperature of the hot-rolled steel sheet to -40°C or less, the movement of dislocations introduced in the pipe-making process can be suppressed, dislocation entanglement can be prevented, and dislocations can remain as movable dislocations. That is, dislocations introduced into the grains are uniformly distributed, so the A value becomes large.
[0171] When the temperature of the hot-rolled steel sheet in the pipe-making process exceeds -40°C, dislocations introduced in the pipe-making process are easy to move, so dislocations are easy to entangle with each other and form cells, and the number of movable dislocations decreases. The temperature of the hot-rolled steel sheet in the pipe-making process is more preferably -50°C or less, and further preferably -55°C or less.
[0172] The lower limit of the temperature of the hot-rolled steel sheet in the pipe-making process is not particularly specified, but is preferably -90°C or higher, and more preferably -80°C or higher, from the viewpoints of increased pipe-making load due to increased deformation resistance of the hot-rolled steel sheet, temperature management of hydraulic devices, etc., and cooling cost.
[0173] Upsetting amount during resistance welding (optimal conditions)
[0174] The upset amount during resistance welding is controlled in such a way that inclusions such as oxides and nitrides that reduce toughness can be discharged together with the molten steel. The upset amount is preferably set to 20% or more of the plate thickness. However, when the upset amount exceeds 100% of the plate thickness, the squeeze roll load becomes large. Therefore, the upset amount is preferably controlled within the range of 20% or more of the plate thickness and 100% or less of the plate thickness. More preferably, it is 40% or more of the plate thickness. More preferably, it is 80% or less of the plate thickness.
[0175] The upset amount is determined as the difference between the outer circumference of the steel pipe (open pipe) before electric resistance welding and the outer circumference of the steel pipe after electric resistance welding.
[0176] [Sizing process]
[0177] The shrinking temperature of the steel pipe raw material: below -40℃
[0178] In the sizing step after resistance welding, the steel pipe material is reduced in diameter at -40°C or below by rollers (sizing rollers) arranged above, below, and on the left and right sides of the steel pipe material, and the outer diameter and roundness are adjusted to desired values.
[0179] The cooling method of the electric resistance welded steel pipe in the sizing process includes, for example, a method of continuously performing the sizing process immediately after the pipe making process performed by cooling to a temperature of -40°C or less as described above, and a method of further cooling the electric resistance welded steel pipe after the pipe making process and performing the sizing process. In addition, a part of the equipment in the sizing process may be cooled to -40°C or less.
[0180] By keeping the temperature of the electric resistance welded steel pipe before the sizing step below -40°C, the movement of dislocations introduced in the sizing step can be suppressed, the dislocations can be prevented from being entangled, and can remain as movable dislocations. That is, the dislocations introduced into the grains are evenly distributed, so the A value becomes larger.
[0181] When the temperature of the electric resistance welded steel pipe in the sizing process exceeds -40°C, the dislocations introduced in the sizing process are easy to move, so the dislocations are easy to entangle with each other and form cells, and the number of movable dislocations decreases. The temperature of the electric resistance welded steel pipe in the sizing process is more preferably -50°C or less, and further preferably -55°C or less.
[0182] The lower limit of the temperature of the electric resistance welded steel pipe in the sizing step is not particularly specified, but is preferably -90°C or higher, and more preferably -80°C or higher, from the viewpoints of increased sizing load due to increased deformation resistance of the electric resistance welded steel pipe, temperature management of hydraulic devices, etc., and cooling cost.
[0183] Diameter reduction ratio (preferred condition)
[0184] In order to improve the outer diameter accuracy and roundness, it is preferred to reduce the steel pipe diameter in the sizing process so that the steel pipe circumference is reduced by a total ratio of 0.5% or more. However, when the steel pipe diameter is reduced so that the steel pipe circumference is reduced by a total ratio of more than 4.0%, the bending amount in the pipe axis direction when the roller passes becomes larger, and the yield ratio increases. Therefore, it is preferred to reduce the steel pipe diameter so that the steel pipe circumference is reduced by a ratio of 0.5% or more and 4.0% or less. The ratio is more preferably 1.0% or more. In addition, the ratio is more preferably 3.0% or less.
[0185] It should be noted that in the sizing process after resistance welding, the yield ratio is suppressed by minimizing the amount of bending in the pipe axis direction when the steel pipe raw material passes through the sizing roller. Therefore, it is preferred to use two or more sizing stands to perform two or more stages of diameter reduction, and the diameter reduction of each sizing stand is preferably performed in a manner that the pipe circumference is reduced by a ratio of 1.0% or less when the adjacent sizing stands are compared. In addition, the ratio is preferably 0.50% or more.
[0186] The electric resistance welded steel pipe of the present invention is manufactured by the method for manufacturing an electric resistance welded steel pipe described above.
[0187] As described above, the method for producing an electric-resistance-welded steel pipe of the present invention can also be applied to a thick-walled material having a base material portion having a wall thickness in the range of 15 mm to 30 mm.
[0188] Here, whether the steel pipe is an electric resistance welded steel pipe can be judged as follows. Cut the electric resistance welded steel pipe perpendicular to the pipe axis direction, grind the cut surface including the weld (resistance weld), etch it with a corrosive liquid, and observe it with an optical microscope. If the width of the molten solidified part of the weld (resistance weld) in the pipe circumferential direction is greater than 1.0 μm and less than 1000 μm in the entire thickness of the pipe, it is an electric resistance welded steel pipe. It should be noted that the corrosive liquid can be selected appropriately according to the steel composition and the type of steel pipe.
[0189] use Figure 1 The welded portion (resistance welded portion) will be further described. Figure 1 This is a circumferential cross-sectional view of the weld and its surrounding area, showing the state after the cut surface including the weld has been ground and etched. Figure 1 As shown, the molten solidified portion 3 can be observed as a region having a different structure and contrast from the base material portion 1 and the weld heat affected zone 2. For example, the molten solidified portion 3 of the electric resistance welded steel pipe of carbon steel and low alloy steel can be specified as a region observed relatively white using an optical microscope in the above cross section after etching with nital.
[0190] Example
[0191] Hereinafter, the present invention will be described in more detail based on examples. It should be noted that the present invention is not limited to the following examples.
[0192] Molten steel having the component composition shown in Table 1 was melted to produce slabs (steel raw materials). The obtained slabs were subjected to hot rolling, cooling and coiling under the conditions shown in Table 2 to produce hot-rolled steel sheets (hot-rolled steel sheets for electric resistance welded steel pipes).
[0193] After the coiling process, the hot-rolled steel sheet cooled to the temperature shown in Table 2 is formed into a cylindrical open tube (round steel tube) by roll forming, and the butt joint of the open tube is subjected to electric resistance welding to obtain a steel tube raw material (tube making process). Next, the steel tube raw material is reduced in diameter at the temperature shown in Table 2 (sizing process) to obtain an electric resistance welded steel tube having an outer diameter D (mm) and a wall thickness t (mm) shown in Table 2.
[0194] Various test pieces were cut from the obtained electric resistance welded steel pipe, and dislocation analysis, structure analysis, tensile test, and Charpy impact test were performed by the following methods. Here, various test pieces were cut from the base material portion which was 90° away from the electric resistance weld portion in the pipe circumferential direction when the electric resistance weld portion was set to 0°.
[0195] [Dislocation Analysis]
[0196] Regarding the dislocation density ρ, after mirror polishing the cross section parallel to both the tube length direction and the wall thickness direction, electrolytic polishing of 100 μm was performed to remove the surface processing layer, and a test piece was prepared in such a way that the diffraction surface was the center of the wall thickness. The test piece was used for X-ray diffraction, and the modified Williamson-Hall method and the modified Warren-Averbach method (references 1 and 2 above) were used to obtain the dislocation density ρ. The X-ray source used CuKα rays. The tube voltage was set to 45 kV and the tube current was set to 200 mA.
[0197] The parameter φ was obtained from the above X-ray diffraction results using the direct fitting / corrected Williamson-Hall method (reference 3 above). The various constants required in the direct fitting / corrected Williamson-Hall method (reference 3 above) were set to Γ0=0.261, C h00 S =0.298, C h00 E =0.262, q s =2.652,q e =1.372.
[0198] The Burgers vector b of the dislocation is set to 0.248×10 -9 m.
[0199] The obtained dislocation density ρ, parameter φ, the Burgers vector b of the dislocation, and equation (1) are used to determine the A value related to the distribution state of the dislocation.
[0200] A=φ / ((πρ / 2) 1 / 2 ×b)…(1)
[0201] Table 3 shows the values obtained respectively.
[0202] [Organizational Analysis]
[0203] The test piece for tissue analysis was cut so that the observation surface was a cross section parallel to both the tube length direction and the wall thickness direction and the center of the wall thickness, mirror polished, and then etched with nital to prepare the test piece for tissue analysis. The tissue analysis was performed using an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) to observe and photograph the structure of the center of the wall thickness.
[0204] The area ratios of ferrite, bainite, pearlite, and the remainder (martensite, austenite) were calculated from the obtained optical microscope images and SEM images. The area ratio of each structure was observed in more than 5 fields of view and calculated as the average value of the values obtained in each field of view. Here, the area ratio obtained by the structure analysis was used as the volume ratio of each structure.
[0205] It should be noted that martensite and austenite are difficult to identify in optical microscope images and SEM images, so the area ratio of the structure observed in the form of martensite or austenite is measured based on the obtained SEM image, and the value obtained by subtracting the volume ratio of austenite measured by the method described later from the measured value is used as the volume ratio of martensite.
[0206] The volume fraction of austenite is measured by X-ray diffraction using a test piece made in the same way as the test piece for dislocation analysis. The volume fraction of austenite is obtained from the integrated intensity of the (200), (220), (311) planes of fcc iron and the (200), (211) planes of bcc iron using Mo Kα rays. In addition, the volume fraction of the bcc phase is also obtained at the same time.
[0207] In addition, the mensuration of average crystal grain size is carried out as follows.First, utilize SEM / EBSD method, calculate the histogram of crystal grain size distribution (the horizontal axis is set to crystal grain size, the vertical axis is set to the figure of the existence ratio in each crystal grain size), obtain the arithmetic mean of crystal grain size.Specifically, about crystal grain size, obtain the orientation difference between adjacent crystal grains, the orientation difference is that the boundary more than 15 ° is set to crystal grain (grain boundary), measure the equivalent circle diameter of crystal grain.Use average equivalent circle diameter as average crystal grain size.Here, equivalent circle diameter refers to the diameter of the circle that area is equal to the crystal grain as object.
[0208] The measurement conditions are set as acceleration voltage: 15 kV, measurement area: 500 μm×500 μm, and measurement step length: 0.5 μm. It should be noted that in the grain size analysis, crystals with a grain size of less than 2.0 μm are excluded from the analysis object as measurement noise, and the obtained area ratio is equal to the volume ratio.
[0209] Table 3 shows the obtained results respectively.
[0210] [Tensile test]
[0211] In the tensile test, a JIS No. 5 tensile test piece was cut so that the tensile direction was parallel to the longitudinal direction of the tube, and the test was carried out in accordance with the provisions of JIS Z 2241. The yield stress YS (MPa) and the tensile strength TS (MPa) were measured, and the yield ratio YR (%) defined by (YS / TS) × 100 was calculated. The yield stress YS was set to the flow stress at a nominal strain of 0.5%.
[0212] Table 4 shows the obtained results respectively.
[0213] [Charpy impact test]
[0214] In the Charpy impact test, a V-notch test piece is cut from the center of the wall thickness of the electric resistance welded steel pipe so that the length direction of the test piece is parallel to the length direction of the pipe. The test is carried out at -40°C in accordance with the provisions of JIS Z 2242, and the absorbed energy (J) is calculated. The number of test pieces is set to 3 each, and the average value of their absorbed energy is taken as the absorbed energy of the electric resistance welded steel pipe.
[0215] Table 4 shows the obtained results.
[0216]
[0217]
[0218]
[0219] [Table 4]
[0220]
[0221] In Tables 3 and 4, Steel Pipes Nos. 1 to 5, 12, 13, and 19 to 22 are examples of the present invention, and Steel Pipes Nos. 6 to 11 and 14 to 18 are comparative examples.
[0222] The electric resistance welded steel pipes of the examples of the present invention all had a steel structure of a base material portion having a volume fraction of bcc phase of 80% or more, an average grain size of 15.0 μm or less, and an A value of 0.55 or more and 0.85 or less. In addition, the mechanical properties of the electric resistance welded steel pipes of the examples of the present invention all had a yield ratio of 90% or less and a Charpy absorbed energy of 100 J or more at -40°C.
[0223] Explanation of symbols
[0224] 1. Parent material
[0225] 2 Welding heat affected zone
[0226] 3 Melting and solidification section
Claims
1. An electric resistance welded steel pipe, comprising a base material portion and a weld portion, wherein: The base material portion has a composition, in mass%, of C: 0.001% to 0.30%, Si: 0.01% to 2.0%, Mn: 0.20% to 3.0%, P: 0.050% to 0.020%, Al: 0.005% to 0.10%, N: 0.010% to 0.15%, and the balance is Fe and unavoidable impurities. In the steel structure of the center portion of the wall thickness of the base material portion, The volume fraction of the bcc phase is 80% or more. The total volume fraction of ferrite and bainite is 85% or more. The average crystal grain size is less than 15.0 μm. The A value represented by the formula (1) is 0.55 or more and 0.85 or less. The yield ratio in the pipe axis direction is less than 90%. The Charpy absorbed energy of the base material portion at -40°C is 100 J or more, A=φ / ((pr / 2) 1 / 2 ×b)…(1) Here, in formula (1), φ: a parameter indicating the degree of processing obtained by X-ray diffraction, ρ: dislocation density, its unit is m -2 , b: Burgers vector of dislocation, in m, π: Pi.
2. The electric resistance welded steel pipe according to claim 1, wherein: In addition to the above-mentioned component composition, it also contains, in terms of mass%, one or more selected from the group consisting of Cu: less than 1.0%, Ni: less than 1.0%, Cr: less than 1.0%, Mo: less than 1.0%, Nb: less than 0.15%, V: less than 0.15%, Ca: less than 0.010%, and B: less than 0.010%.
3. The electric resistance welded steel pipe according to claim 1 or 2, wherein: The wall thickness of the base material portion is greater than or equal to 15 mm and less than or equal to 30 mm.
4. A method for manufacturing an electric resistance welded steel pipe, which is the method for manufacturing an electric resistance welded steel pipe according to any one of claims 1 to 3, comprising: A hot rolling process of heating a steel material to a heating temperature of 1100° C. to 1300° C., and then hot rolling the steel material under the conditions of a rough rolling end temperature of 850° C. to 1150° C., a finish rolling end temperature of 750° C. to 900° C., and a total reduction ratio of 50% or more at 930° C. to obtain a hot-rolled sheet; A cooling step of cooling the hot rolled sheet at an average cooling rate of 5°C / s to 30°C / s and a cooling stop temperature of 400°C to 650°C, based on the sheet thickness center temperature; A coiling step of coiling the hot-rolled sheet at a temperature of 400° C. to 650° C. to obtain a hot-rolled steel sheet; a pipe making step of forming the hot-rolled steel sheet into a cylindrical shape at a temperature of -40°C or less by roll forming and performing electric resistance welding to make a steel pipe raw material; and The steel pipe raw material is reduced in diameter at a temperature below -40°C to obtain a sizing step of electric resistance welded steel pipe, in, The steel material has a component composition, in mass %, of C: 0.001% to 0.30%, Si: 0.01% to 2.0%, Mn: 0.20% to 3.0%, P: 0.050% to 0.020%, Al: 0.005% to 0.10%, N: 0.010% to 0.15%, and the balance is Fe and unavoidable impurities.
5. The method for manufacturing an electric resistance welded steel pipe according to claim 4, wherein: In addition to the above-mentioned component composition, it also contains, in terms of mass%, one or more selected from the group consisting of Cu: less than 1.0%, Ni: less than 1.0%, Cr: less than 1.0%, Mo: less than 1.0%, Nb: less than 0.15%, V: less than 0.15%, Ca: less than 0.010%, and B: less than 0.010%.
6. The method for manufacturing an electric resistance welded steel pipe according to claim 4 or 5, wherein: The wall thickness of the base material portion of the electric resistance welded steel pipe is 15 mm or more and 30 mm or less.
Citation Information
Patent Citations
Stator windings supporting device
JP1977093903A
Paper discharging device
JP1987060757A
High-strength thick-walled electric-resistance-welded steel pipe having excellent low-temperature toughness, and method for manufacturing same
CN104220622A
Thick-walled electric resistance welded steel pipe for line pipe, and method for manufacturing said steel pipe
CN105378131A