A high-strength and high-release micro-nano cellulose / sodium alginate dressing and its preparation method and application
By combining micro-nano cellulose with sodium alginate and molding it in a calcium ion solution, the problems of poor mechanical properties and weak release ability of hydrogel materials in dressing applications are solved, and a dressing with high strength and high release rate is achieved. , and the process is environmentally friendly and non-toxic, suitable for medical dressings and cosmetic masks.
Patent Information
- Application Number
- CN202310234076.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-13
AI Technical Summary
Existing hydrogel materials have problems with poor mechanical properties, weak release ability, unfriendly environment and potential toxicity in dressing applications. In particular, sodium alginate has poor mechanical strength, severe shrinkage and poor uniformity after molding.
The method of combining micro-nano cellulose and sodium alginate is used to prepare high-strength micro-nano cellulose/sodium alginate dressing through the steps of loosening, centrifugation, grinding, and homogenization. The micro-nano cellulose is used to promote the rapid dissolution of sodium alginate. Shape and reduce shrinkage, and shape in calcium ion solution to form a cross-linked film.
It improves the mechanical strength and release efficiency of the dressing, reduces shrinkage during the molding process, and achieves a dressing with high strength and high release rate. The process is environmentally friendly and non-toxic, and is suitable for medical dressings and cosmetic masks.
Smart Images

Figure CN116236607B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer functional materials, and specifically relates to a high-strength and high-release micro-nano cellulose / sodium alginate dressing and a preparation method and application thereof. Background Art
[0002] Hydrogel is a three-dimensional mesh material with high water retention properties. High water retention can provide sufficient moisture retention and carry sufficient active ingredients, and has received widespread attention in dressing applications. However, hydrogels have poor mechanical properties, weak ability to release active ingredients, and an environmentally unfriendly production process, all of which limit their application in dressings.
[0003] Sodium alginate is a natural polysaccharide extracted from alginic acid. Hydrogel materials based on sodium alginate have good biocompatibility, easy degradation, fast molding speed, and many applications in the medical field. However, the hydrogel after molding has poor mechanical strength, severe shrinkage, and poor uniformity. A non-toxic and bio-friendly method is urgently needed to solve this problem.
[0004] Most existing gels use alkali (such as patent application with application number 202111556373.3) or metal (such as patent application with application number 202211325914.6) as chelating agents, which pollute the environment and may be harmful to the human body. Summary of the invention
[0005] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing. The method uses micro-nano cellulose to promote the rapid molding of sodium alginate and reduce shrinkage. The added micro-nano cellulose film has higher strength and greater release than the pure sodium alginate film. The preparation method solves the problems of complex production, potential toxicity and poor mechanical properties of condensed dressings in the prior art.
[0006] Another object of the present invention is to provide a high-strength and high-release micro-nano cellulose / sodium alginate dressing prepared by the above method.
[0007] Another object of the present invention is to provide an application of the above-mentioned high-strength and high-release micro-nano cellulose / sodium alginate dressing.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing comprises the following steps:
[0010] (1) The plant fibers are first deflated and then centrifuged, then diluted and soaked after centrifugation, and then refined after soaking for a certain period of time;
[0011] (2) diluting the slurry obtained in step (1), and then homogenizing it with a high-pressure homogenizer to obtain a micro-nano cellulose suspension;
[0012] (3) adding sodium alginate and hyaluronic acid to the micro-nanocellulose suspension obtained in step (2), then adding polyvinyl alcohol solution, and stirring to obtain a mixed solution;
[0013] (4) pouring the mixed solution obtained in step (3) into a mold, and then immersing it in a calcium ion solution to form a cross-linked micro-nano cellulose / sodium alginate film, which is the high-strength and high-release micro-nano cellulose / sodium alginate dressing.
[0014] Preferably, the plant fiber in step (1) comprises at least one of softwood fiber, hardwood fiber, grass fiber, bast fiber, seed hair fiber and leaf fiber. In the present invention, softwood fiber is preferred.
[0015] Preferably, the centrifugal speed in step (1) is 3000-10000 r / min, and the centrifugal time is 10-30 min.
[0016] Preferably, the dilution in step (1) refers to diluting the softwood fiber to 7-15 wt%.
[0017] Preferably, the soaking time in step (1) is 12-24 hours.
[0018] Preferably, the pulping in step (1) refers to processing using a PFI pulping machine with a pulping speed of 30,000-100,000 rpm for cutting and microfibrillating coniferous wood fibers.
[0019] Preferably, in step (2), the slurry is diluted to a fiber concentration of 0.1-1.5 wt %; and the homogenization is performed 5-30 times.
[0020] Preferably, the micro-nano fibers in step (2) have a width of 10 nm to 100 nm and an aspect ratio greater than 100.
[0021] Preferably, after the homogenization in step (2), the process further comprises rotary evaporating the suspension at 40° C., 2000 Pa low vacuum and 180 r / min until the concentration of the micro-nano cellulose is 0.8 wt %.
[0022] Preferably, in the mixed solution of step (3), the concentration of micro-nano cellulose is 0.3-1.5wt%, the concentration of sodium alginate is 1-3wt%, the concentration of hyaluronic acid is 0.1-0.25wt%, and the concentration of polyvinyl alcohol is 1wt%.
[0023] Preferably, the concentration of the polyvinyl alcohol solution in step (3) is 5-20 wt%.
[0024] Preferably, in step (4), the mixed liquid is first vacuum degassed and then poured into the mold.
[0025] Further preferably, the vacuum degassing is carried out at 0.1 MPa.
[0026] Preferably, the concentration of the calcium ion solution in step (4) is 0.5-2wt%, and the molding time is 5-20min.
[0027] Preferably, the calcium ion solution in step (4) includes calcium chloride, calcium sulfate or calcium lactate.
[0028] The high-strength and high-release micro-nano cellulose / sodium alginate dressing of the present invention has a strength of 40-140 Kpa, an elongation of 70-260%, and a release rate of more than 50% within one hour.
[0029] The high-strength and high-release micro-nano cellulose / sodium alginate dressing of the present invention can be applied to medical dressings and cosmetic facial masks.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] (1) The materials used in the present invention are cheap and abundant. Cellulose is the most abundant polysaccharide in the world, and sodium alginate is a natural polysaccharide extracted from marine plants. It has the characteristics of biodegradability and good biocompatibility. The prepared materials have a very wide range of application scenarios.
[0032] (2) The micro-nanocellulose with high aspect ratio prepared by mechanical method has the characteristics of high specific surface area, high strength and low density. At the same time, the surface contains abundant hydroxyl groups, which can form hydrogen bonds with alginate. It not only significantly improves the strength of sodium alginate film, promotes its molding in calcium ion solution, reduces the shrinkage of the film during the molding process, but also increases the release efficiency of the film, which is very important for dressings.
[0033] (3) The preparation method of the present invention is easy to operate, does not produce waste chemicals, is environmentally friendly, and can be easily industrialized. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is an electron microscope image of the cellulose raw material used in Example 1.
[0035] Figure 2 This is an electron microscope image of the micro-nanocellulose prepared in Example 1.
[0036] Figure 3 Different micro-nanocellulose (CNF), polyvinyl alcohol (PVA) and sodium alginate were immersed in different concentrations of CaCl2 to observe their shrinkage during the molding process.
[0037] Figure 4 The tensile strength test method in the figure is: film width 10mm, film length 30mm, tensile speed 1mm / min.
[0038] Figure 5 This is a picture of a CNF / SA-0.5wt% film repeatedly stretched four times. The tensile strength test method in the figure is as follows: the film width is 10mm, the film length is 30mm, the stretching speed is 1mm / min, the first stretching, the elongation is 30% and then returns to the original position, and then the second stretching is performed, stretching to an elongation of 60% and returning to the original position. It broke during the third stretching. In the figure, CNF / SA-0.5wt%-1 refers to the first stretching, CNF / SA-0.5wt%-2 refers to the second stretching, and CNF / SA-0.5wt%-3 refers to the third stretching.
[0039] Figure 6 This is a picture of a CNF / PVA / SA-0.5wt% film repeatedly stretched four times. The tensile strength test method in the figure is as follows: the film width is 10mm, the film length is 30mm, the stretching speed is 1mm / min, the first stretching, the elongation is 30% and then returns to the original position, and then the second stretching is performed, and the elongation is stretched to 60% and returns to the original position. The third stretching broke during the process, and the elongation was stretched to 90% and returned to the original position, and the fourth stretching broke. In the figure, CNF / PVA / SA-0.5wt%-1 refers to the first stretching, CNF / PVA / SA-0.5wt%-2 refers to the second stretching, CNF / PVA / SA-0.5wt%-3 refers to the third stretching, and CNF / PVA / SA-0.5wt%-4 refers to the fourth stretching. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. The raw materials involved in the present invention can be purchased directly from the market. For process parameters not particularly noted, conventional techniques can be used.
[0041] Example 1
[0042] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0043] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0044] Step (3): Weigh 5 g of polyvinyl alcohol and add it to 45 g of water. Stir at 200 r / min for half an hour in a 98° C. water bath to obtain a completely dissolved polyvinyl alcohol solution.
[0045] 1.8 g of sodium alginate and 0.1 g of hyaluronic acid were weighed and dissolved in 100 ml of 0.8 wt% micro-nanocellulose suspension and stirred evenly at room temperature. Then 10 g of polyvinyl alcohol solution was weighed and added to the micro-nanocellulose suspension and stirred at 200 r / min for 1 h to obtain a mixed suspension. The obtained liquid was subjected to vacuum degassing at 0.1 MPa.
[0046] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, which is numbered CNF / SA / PVA-0.5 wt %.
[0047] Example 2
[0048] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0049] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0050] Step (3): Weigh 5 g of polyvinyl alcohol and add it to 45 g of water. Stir at 200 r / min for half an hour in a water bath at 100° C. to obtain a completely dissolved polyvinyl alcohol solution.
[0051] 1.5 g of sodium alginate and 0.1 g of hyaluronic acid were weighed and dissolved in 100 ml of 0.8 wt% micro-nanocellulose suspension and stirred evenly at room temperature. Then 10 g of polyvinyl alcohol solution was weighed and added to the micro-nanocellulose suspension and stirred at 200 r / min for 1 h to obtain a mixed suspension. The obtained liquid was subjected to vacuum degassing at 0.1 MPa.
[0052] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 1 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, and record the sample number as CNF / SA / PVA-1wt%.
[0053] Example 3
[0054] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0055] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0056] Step (3): Weigh 5 g of polyvinyl alcohol and add it to 45 g of water. Stir at 200 r / min for half an hour in a water bath at 100° C. to obtain a completely dissolved polyvinyl alcohol solution.
[0057] 1.5g sodium alginate and 0.1g tetracycline hydrochloride were weighed and dissolved in 100ml of 0.8wt% micro-nanocellulose suspension, and stirred evenly at room temperature. Then 10g polyvinyl alcohol solution was weighed and added into the micro-nanocellulose suspension, and stirred at 200r / min for 1h to obtain a mixed suspension. The obtained liquid was subjected to vacuum degassing at 0.1MPa.
[0058] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 1 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, and record the sample number CNF / SA / PVA-0.5 wt %-T.
[0059] Example 4
[0060] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0061] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0062] Step (3): Weigh 5 g of polyvinyl alcohol and add it to 45 g of water. Stir at 200 r / min for half an hour in a water bath at 100° C. to obtain a completely dissolved polyvinyl alcohol solution.
[0063] Weigh 1.5g of sodium alginate and 0.1g of collagen and dissolve them in 100ml of 0.8wt% micro-nanocellulose suspension, and stir them evenly at room temperature. Then weigh 10g of the polyvinyl alcohol solution in step 2, add it into the micro-nanocellulose suspension, and stir at 200r / min for 1h to obtain a mixed suspension. The obtained liquid is subjected to vacuum degassing at 0.1MPa.
[0064] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film CNF / SA / PVA-0.5 wt %-C.
[0065] Example 5
[0066] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0067] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0068] Step (3): Weigh 5 g of polyvinyl alcohol and add it to 45 g of water. Stir at 200 r / min for half an hour in a water bath at 100° C. to obtain a completely dissolved polyvinyl alcohol solution.
[0069] 1.5 g of sodium alginate and 0.1 g of hyaluronic acid were weighed and dissolved in 100 ml of 0.8 wt% micro-nanocellulose suspension and stirred evenly at room temperature. Then 10 g of polyvinyl alcohol solution was weighed and added to the micro-nanocellulose suspension and stirred at 200 r / min for 1 h to obtain a mixed suspension. The obtained liquid was subjected to vacuum degassing at 0.1 MPa.
[0070] Step (4): Pour 6 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 1 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, which is numbered CNF / SA (1.5%) / PVA-1 wt %.
[0071] Comparative Example 1
[0072] Polyvinyl alcohol and sodium alginate films without micro-nanocellulose were used as controls to observe the shrinkage and strength changes of the films.
[0073] Step (1): Weigh 7.5 g of polyvinyl alcohol and add it to 42.5 g of water. Stir at 200 r / min for 1 hour in a 98° C. water bath to obtain a completely dissolved polyvinyl alcohol solution.
[0074] Step (2): Weigh 1.8 g of sodium alginate and 0.1 g of hyaluronic acid and dissolve them in 100 ml of pure water, and stir them evenly at room temperature. Then weigh 10 g of polyvinyl alcohol solution and add it into the solution, and stir at 200 r / min for 1 hour to obtain a mixed suspension. The obtained liquid is subjected to vacuum degassing at 0.1 MPa.
[0075] Step (3): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, which is numbered as SA / PVA-0.5 wt %.
[0076] Comparative Example 2
[0077] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0078] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0079] Step (3): Weigh 1.5 g of sodium alginate and 0.1 g of hyaluronic acid and dissolve them in 100 ml of 0.8 wt% micro-nanocellulose suspension, stir evenly at room temperature, and perform vacuum degassing at 0.1 MPa on the obtained liquid.
[0080] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 1 wt % calcium chloride solution for 10 min to obtain a completely cross-linked micro-nano cellulose / sodium alginate film, and record the sample number as CNF / SA-1 wt %.
[0081] Comparative Example 3
[0082] Micro-nanocellulose and sodium alginate films without polyvinyl alcohol were used as controls to observe the shrinkage and strength changes of the films.
[0083] Step (1): The softwood fiber was pre-pulped by a Valley beater, centrifuged at 4000 r / min for 15 min, the obtained softwood fiber was diluted to 10 wt%, and soaked for 12 h; the softwood fiber was processed by a PFI refiner at a refining speed of 60,000 r .
[0084] Step (2): dilute the obtained fiber to a fiber concentration of 0.3wt%, and homogenize it 5 times with a high-pressure homogenizer to obtain uniform and fine micro-nano cellulose. The diameter of the micro-nano cellulose is 20-50nm, and the aspect ratio is 150-200. The micro-nano cellulose is rotary evaporated at 40°C, 2000Pa low vacuum, and 180r / min to a concentration of 0.8wt%.
[0085] Step (3): Weigh 1.8 g of sodium alginate and 0.1 g of hyaluronic acid and dissolve them in 100 ml of 0.8 wt% micro-nanocellulose suspension, stir evenly at room temperature, and perform vacuum degassing at 0.1 MPa on the obtained liquid.
[0086] Step (4): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, which is numbered CNF / SA-0.5 wt %.
[0087] Comparative Example 4
[0088] The sodium alginate film without polyvinyl alcohol and micro-nanocellulose was used as a control to observe the film shrinkage and strength changes.
[0089] Step (1): Weigh 1.8 g of sodium alginate and 0.1 g of hyaluronic acid and dissolve them in 100 ml of pure water, stir them evenly at room temperature, and perform vacuum degassing at 0.1 MPa on the resulting liquid.
[0090] Step (2): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked micro-nano cellulose / sodium alginate film, which is numbered SA-0.5 wt %.
[0091] Comparative Example 5
[0092] The release of tetracycline hydrochloride was observed using polyvinyl alcohol and sodium alginate films without micro-nanocellulose as controls.
[0093] Step (1): Weigh 7.5 g of polyvinyl alcohol and add it to 42.5 g of water. Stir at 200 r / min for 1 hour in a 98° C. water bath to obtain a completely dissolved polyvinyl alcohol solution.
[0094] Step (2): Weigh 1.8 g of sodium alginate and 0.1 g of hyaluronic acid and dissolve them in 100 ml of pure water, and stir them evenly at room temperature. Then weigh 10 g of polyvinyl alcohol solution and add it into the solution, and stir at 200 r / min for 1 hour to obtain a mixed suspension. The obtained liquid is subjected to vacuum degassing at 0.1 MPa.
[0095] Step (3): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt % calcium chloride solution for 10 min to obtain a cross-linked polyvinyl alcohol / sodium alginate film, denoted as SA / PVA-0.5 wt %-T.
[0096] Comparative Example 6
[0097] The release of collagen was observed using polyvinyl alcohol and sodium alginate membranes without micro-nanocellulose as controls.
[0098] Step (1): Weigh 7.5 g of polyvinyl alcohol and add it to 42.5 g of water. Stir at 200 r / min for 1 hour in a 98° C. water bath to obtain a dissolved polyvinyl alcohol solution.
[0099] Step (2): Weigh 1.8 g of sodium alginate and 0.1 g of collagen and dissolve them in 100 ml of pure water, and stir them evenly at room temperature. Then weigh 10 g of polyvinyl alcohol solution and add it into the solution, and stir at 200 r / min for 1 hour to obtain a mixed suspension. The obtained liquid is subjected to vacuum degassing at 0.1 MPa.
[0100] Step (3): Pour 9 g of the vacuum degassed liquid into a culture dish with a diameter of 8.5 cm, and slowly immerse the culture dish in a 0.5 wt% calcium chloride solution for 10 min to obtain a cross-linked polyvinyl alcohol / sodium alginate film, which is numbered SA / PVA-0.5 wt%-C.
[0101] (I) In order to evaluate the release of active ingredients by the membrane, tetracycline hydrochloride was used to simulate the release of active ingredients. The sample was placed in 100 ml PBS buffer, and the sample was shaken at a rate of 50 r / min on an air shaker. 4 ml of sustained-release solution was taken at 15, 30, 45 and 60 min, respectively, and detected at a wavelength of 360 nm using a UV-visible spectrophotometer. As described in Table 1, the release amount in the first 1 h was close to or even exceeded 50%, while in Comparative Example 2, the sample without CNF had a release rate of only 38.29% in 1 h. The release performance of the sample without the addition of nanocellulose was significantly improved.
[0102] Table 1 shows the release of tetracycline hydrochloride from two parallel samples of the sample CNF / SA / PVA-0.5wt%-T obtained in Example 3 and the sample SA / PVA-0.5wt%-T obtained in Comparative Example 5.
[0103]
[0104] (ii) In order to further evaluate the release of different components by the membrane, collagen was used to simulate the release of active ingredients. The sample was placed in 100ml PBS buffer, and the sample was shaken at a rate of 50r / min on an air shaker. 4ml of sustained-release solution was taken at 15, 30, 45 and 60min, respectively, and detected at a wavelength of 230nm using a UV-visible spectrophotometer. As described in Table 2, the release amount in the first 1h has exceeded 50%, and the release effect is excellent. The release rate was studied with Comparative Example 6, but when the PVA / SA without nanofibers was soaked in water, the sample was broken and could not be used.
[0105] Table 2 Collagen release of two parallel samples of the sample obtained in Example 4 - CNF / SA / PVA-0.5wt%-C
[0106]
[0107] (three) Figure 3The shrinkage of the membranes during the preparation of six mixed membranes was shown. The positive effect of adding micro-nanocellulose and polyvinyl alcohol on the shrinkage of membrane molding, as well as the effect of calcium ion concentration on the shrinkage of membranes during molding, were investigated. Figure 3 The situation expressed is described in detail. The pure sodium alginate (SA) film has a shrinkage rate of up to 42.12%, and the molding effect is very poor after 10 minutes of immersion. After adding only polyvinyl alcohol (PVA), the shrinkage rate dropped to 24.12%, but under the same molding conditions, adding micro-nano cellulose (CNF), the shrinkage rate of the film dropped to 18.94%. When adding micro-nano cellulose and polyvinyl alcohol at the same time, the shrinkage rate was only 7.65%, and the surface of the film was smooth and flat. Comparing the molding of 0.5wt% and 1wt% calcium chloride, the 0.5wt% molded film has better strength and toughness.
[0108] Figure 4 The tensile properties of the films formed in different calcium ions described above prove that the film formed with 0.5wt% calcium ions is better. At the same time, the experiment shows that the tensile strength and toughness of the film with added polyvinyl alcohol are lower than those of the film without added polyvinyl alcohol. Figure 5 and Figure 6 The data proves that the addition of polyvinyl alcohol is beneficial to the reorganization of hydrogen bonds during the continuous pulling process, and it has better toughness and strength after repeated stretching.
[0109] Table 3 Shrinkage of different samples in Examples 1, 2 and Comparative Examples 1-4
[0110]
[0111]
[0112] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing, characterized in that The steps include: (1) The plant fibers are first deflated and then centrifuged, diluted and soaked after centrifugation, and then refined after soaking for a certain period of time; (2) diluting the slurry obtained in step (1) to a fiber concentration of 0.1-1.5 wt%, and then homogenizing with a high-pressure homogenizer to obtain a micro-nano cellulose suspension; the homogenization number is 5-30 times; the micro-nano fibers have a width of 10 nm-100 nm and an aspect ratio of greater than 100; (3) adding sodium alginate and hyaluronic acid to the micro-nano cellulose suspension obtained in step (2), and then adding polyvinyl alcohol solution, stirring evenly to obtain a mixed solution; in the mixed solution: the concentration of micro-nano cellulose is 0.3-1.5wt%, the concentration of sodium alginate is 1-3wt%, the concentration of hyaluronic acid is 0.1-0.25wt%, and the concentration of polyvinyl alcohol is 1wt%; (4) pouring the mixed solution obtained in step (3) into a mold, and then immersing it in a calcium ion solution for molding, wherein the concentration of the calcium ion solution is 0.5-2wt%, to obtain the high-strength and high-release micro-nano cellulose / sodium alginate dressing.
2. The method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 1, characterized in that: The plant fiber in step (1) comprises at least one of softwood fiber, hardwood fiber, grass fiber, bast fiber, seed hair fiber and leaf fiber; The centrifugal speed in step (1) is 3000-10000 r / min, and the centrifugal time is 10-30 min; The dilution in step (1) refers to diluting the softwood fiber to 7-15 wt %; The soaking time in step (1) is 12-24 hours; The refining in step (1) refers to processing using a PFI refiner with a refining speed of 30,000-100,000 r.
3. The method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 1, characterized in that: After the homogenization in step (2), the suspension is rotary evaporated at 40° C., 2000 Pa low vacuum, and 180 r / min until the concentration of the micro-nano cellulose is 0.8 wt %.
4. The method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 1, characterized in that: In step (4), the mixed liquid is first subjected to vacuum degassing and then poured into a mold.
5. The method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 1, characterized in that: The molding time in step (4) is 5-20 minutes.
6. The method for preparing a high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 1, characterized in that: The calcium ion solution in step (4) includes calcium chloride, calcium sulfate or calcium lactate.
7. A high-strength and high-release micro-nanocellulose / sodium alginate dressing, characterized in that: The invention is prepared by the method according to any one of claims 1 to 6.
8. Use of the high-strength and high-release micro-nano cellulose / sodium alginate dressing according to claim 7 in the preparation of medical dressings or cosmetic facial masks.