Polyurethane ceiling material resistant to moisture and heat deformation and preparation method thereof

By adding melamine and foam stabilizer to the formula of polyurethane ceiling materials, the problem of poor dimensional stability of automobile ceiling materials under high temperature and high humidity conditions is solved, and the high porosity and flame retardant performance of the material is improved, ensuring that the material is Stability and safety in hot environments.

CN116239750BActive Publication Date: 2024-12-06JIANGSU CHANGSHUN POLYMER MATERIAL INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111491939.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-08
Publication Date
2024-12-06
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

Existing automotive ceiling materials are prone to separation, degumming, cracking, and wrinkling problems between the PU foam sheet and the composite layer material under high temperature and high humidity conditions, resulting in poor dimensional stability and affecting the quality of the finished product.

Method used

Using specific polyether polyols and isocyanate formulas, melamine and foam stabilizers are added, and by adjusting the foaming formula and preparation process, a polyurethane ceiling material that is resistant to moisture and heat deformation is prepared to improve the dimensional stability and flame retardant properties of the material.

Benefits of technology

It significantly improves the dimensional stability, porosity and flame retardant properties of polyurethane foam, reduces deformation under high temperature and high humidity conditions, and ensures the stability and safety of the material in hot environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000007935000000031
    Figure GHA0000007935000000031
  • Figure GHA0000007935000000041
    Figure GHA0000007935000000041
  • Figure GHA0000007935000000051
    Figure GHA0000007935000000051
Patent Text Reader

Abstract

The present invention relates to a polyurethane ceiling material resistant to moisture and heat deformation and a preparation method thereof, which mainly solves the peeling or wrinkling phenomenon between the bare PU board and the composite layer caused by the shrinkage of the polyurethane ceiling material in a humid and hot environment in the prior art. The present invention provides a polyurethane ceiling material resistant to moisture and heat deformation, which is composed of component I, component II and component III, and the weight ratio of component I: component II: component III is 100:100-200:5-15; wherein, in parts by weight, component I is composed of the following components: polyether polyol I: 30-40 parts, polyether polyol II: 15-30 parts, polyether polyol III: 30-45 parts, chain extender: 2-6 parts, foam stabilizer: 0.5-2.0 parts, catalyst: 0.2-0.7 parts, water: 2-5 parts; component II: 100-200 parts of isocyanate; component III: 5-15 parts of melamine and the technical scheme of the preparation method thereof, which solves the problem well and can be used in industrial applications of automobile ceiling materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyurethane ceiling material resistant to moisture and heat deformation and a preparation method thereof. Background Art

[0002] As an important part of the interior decoration of the whole vehicle, the car roof material occupies a large interior space in the car. The car roof material with excellent performance is very important. The car roof material is made of polyurethane ceiling PU board and composite layer through a composite process. In modern technology, it is generally divided into two composite processes: dry process and wet process, and the lower density PU foam sheet usually adopts the wet process. In the wet process composite process, the mold temperature is generally in the range of 130-140℃, which requires the PU foam sheet to have good dimensional stability under such high temperature conditions and not easy to shrink and deform, otherwise it will cause the final car roof composite sheet to be formed with deviations. In addition, in the process of vehicle application, under high temperature and high humidity conditions (such as summer or rainy season, etc.), if the dimensional stability is poor, it will cause separation, degumming, cracking, wrinkles and other serious problems between the PU foam sheet and the composite layer material.

[0003] In the current automotive ceiling industry, few people have studied the dimensional stability of polyurethane PU sheets under high temperature and high humidity conditions, and there are few relevant literature and materials. Through simulation and analysis of the wet composite process conditions of various domestic companies, the high temperature and high humidity environment is simulated and set to 120℃, 100% RH (humidity) for 5 hours, 70℃ drying for 3 hours, and this cycle is repeated 3 times. Under this condition, the density is 25-35kg / m 3 The size change rate of domestic polyurethane PU sheets is usually above 5%, and a few can be stabilized within 3-5%. However, sheets with a size change rate of 3-5% will still have serious problems such as separation, degumming, cracking, and wrinkling between the PU foam sheet and the composite layer material in the hot summer. Therefore, the present invention provides a polyurethane ceiling material resistant to moisture and heat deformation and a preparation method thereof by adjusting the formula and the foaming method of the PU sheet.

[0004] Chinese patent CN102391640A discloses a one-step wet PU board for automobile ceilings, which is characterized in that it is made of the following raw materials in weight ratio: 100 parts of a mixture of polyether polyol and polyester polyol, 1-3 parts of mixed silicone oil, 0.1-0.5 parts of amine catalyst, 5-20 parts of mixed foaming agent, 0.1-0.3 parts of delayed catalyst, 1.0-2.0 parts of pore opening agent, and is uniformly mixed to form material A, which reacts with 140-175 parts of modified material B to form large foam blocks, and the sliced ​​PU board is used as a one-step wet automobile ceiling, which has good toughness, high dimensional stability, and low cost. The patent does not disclose specific indicators for dimensional stability. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is that there are problems such as separation, degumming, cracking, wrinkling, etc. between the PU foam sheet and the composite layer material in the wet composite process in the prior art. A new polyurethane ceiling material resistant to moisture and heat deformation is provided, which has the advantages of resistance to moisture and heat deformation, small dimensional change rate, and good flame retardant performance. The second technical problem to be solved by the present invention is to provide a preparation method of a polyurethane ceiling material resistant to moisture and heat deformation corresponding to the first technical problem to be solved.

[0006] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows: a polyurethane ceiling material resistant to moisture and heat deformation, composed of component I, component II and component III, the weight ratio of component I: component II: component III is 100:100-200:5-15; wherein, in parts by weight, component I is composed of the following components: polyether polyol I: 30-40 parts, polyether polyol II: 15-30 parts, polyether polyol III: 30-45 parts, chain extender: 2-6 parts, foam stabilizer: 0.5-2.0 parts, catalyst: 0.2-0.7 parts, water: 2-5 parts; component II: 100-200 parts of isocyanate; component III: 5-15 parts of melamine; wherein, the polyether polyol I uses glycerol as the initiator, and the grafting Propylene oxide is capped with ethylene oxide in an amount of 10% to 25% and a hydroxyl value of 20 to 40 mgKOH / g; the polyether polyol II is prepared by ring-opening polymerization of propylene oxide with one of ethylene glycol, propylene glycol or diethylene glycol as an initiator under the action of a catalyst, and the hydroxyl value is 215 to 350 mgKOH / g; the polyether polyol III is prepared by polymerization of propylene oxide with glycerol as an initiator, and the hydroxyl value is 400 to 540 mgKOH / g; the foam stabilizer is selected from at least one of L580, B8409, HC605, HC580, B8540 or DC193; the catalyst is an amine catalyst, and the isocyanate in component II is selected from one of MDI, TDI or PAPI.

[0007] In the above technical solution, preferably, the amine catalyst is selected from at least one of A33, A1, NE300, ZF10 or LE-710.

[0008] In the above technical solution, preferably, the chain extender is selected from at least one of ethylene glycol, propylene glycol, butylene glycol, glycerol, hexylene glycol, diethylene glycol or dipropylene glycol.

[0009] In the above technical solution, preferably, the isocyanate is selected from at least one of PM-200, M20S, and M50.

[0010] To solve the second of the above technical problems, the technical solution adopted by the present invention is as follows:

[0011] A method for preparing the aforementioned moisture-heat deformation-resistant polyurethane ceiling material comprises the following steps:

[0012] In parts by weight, component I is prepared: (1) In parts by weight, component I is prepared: polyether polyol I: 30-40 parts, polyether polyol II: 15-30 parts, polyether polyol III: 30-45 parts, chain extender: 2-6 parts, foam stabilizer: 0.5-2.0 parts, catalyst: 0.2-0.7 parts, water: 2-5 parts; component II: 100-200 parts of isocyanate; component III: 5-15 parts of melamine; wherein the polyether polyol I is initiator, grafted with propylene oxide, and then capped with ethylene oxide, the capping amount is 10%-25%, and the hydroxyl value is 20-40 mgKOH / g; the polyether polyol II is initiator, such as ethylene glycol, propylene glycol and diethylene glycol, containing active hydrogen groups, and reacts with propylene oxide under the action of a catalyst. The polyol III is prepared by ring-opening polymerization of propylene oxide, with a functionality of 2 and a hydroxyl value of 215-350 mgKOH / g; the polyether polyol III is prepared by polymerization of propylene oxide with propylene glycol as the initiator, with a functionality of 3 and a hydroxyl value of 400-540 mgKOH / g; the foam stabilizer is selected from at least one of L580, B8409, HC605, HC580, B8540 and DC193; the catalyst is an amine catalyst, and the catalyst is preferably an amine catalyst A1, A33 and NE300; the isocyanate in component II is at least one of MDI, TDI or PAPI; the isocyanate in component II is preferably at least one of M2OS, MIPS, PM-200 or M50; the melamine is preferably 80-100 mesh. The weight ratio of component I: component II: component III is 100:100-200:5-15.

[0013] Preparation of component I: according to the components and weight proportions in step (1), weighed polyether polyol I, polyether polyol II, polyether polyol III, foam stabilizer, catalyst, chain extender and water are added to container A in sequence, stirred for 10 to 20 seconds, the material temperature is 19 to 22° C., and mixed thoroughly;

[0014] Preparation of component II:

[0015] According to the components and weight proportions in step (1), the weighed isocyanate of component II is added into container B and stirred evenly. The material temperature is 19-22° C. to prepare component II;

[0016] Preparation of Component III:

[0017] According to the components and weight proportions in step (1), the weighed melamine of component III is added into container C to obtain component III, and the weighed component III is added into component II, and stirred evenly for later use;

[0018] The ambient temperature is controlled at 19-22°C, component I is mixed with a mixture of component II and component III, and after being evenly mixed, the mixture is immediately poured into a foaming box for foaming and then sliced ​​to obtain a polyurethane ceiling material resistant to moisture and heat deformation.

[0019] The technical solution of the present invention has the following advantages: First, by adding melamine to isocyanate in the foaming formula, on the one hand, the support and dimensional stability of the PU sheet can be improved, and the deformation under high temperature and high humidity conditions can be reduced. On the other hand, the material can be endowed with excellent flame retardant properties. Second, the balance between gel and foaming is cleverly matched in the formula, which greatly gives the polyurethane foam the material characteristics of a high open porosity. The shrinkage or expansion caused by the large changes in the external environment of the foam due to closed cells is avoided, and the dimensional stability of the PU sheet is further improved. DETAILED DESCRIPTION

[0020] The present invention will be further described below by way of examples, but is not limited thereto.

[0021] Table 1 List of raw materials

[0022]

[0023]

[0024] [Example 1]

[0025] (1) Prepare the raw materials according to the weight proportions of the following components:

[0026] Component I: 100 parts, specifically including by weight: CHE-2801: 30 parts, CHE-204: 15 parts, CHE-303: 45 parts, L580: 0.7 parts, B8409: 0.3 parts, A1: 0.3 parts, water: 4.7 parts, propylene glycol: 4 parts.

[0027] Component II: 160 parts of isocyanate, specifically including by weight: 60 parts of MIPS, 100 parts of M20S;

[0028] Component II: Melamine specifically includes, by weight: 5 parts of melamine;

[0029] (2) Preparation of Component I:

[0030] According to the weight proportion of component I in step (1), the weighed components are added into container A in sequence, stirred for 15 seconds, the material temperature is 20° C., and mixed thoroughly to prepare component I;

[0031] (3) Preparation of component II:

[0032] According to the weight proportion of component II in step (1), the weighed components are added into container B in sequence, the material temperature is 20° C., and the mixture is mixed thoroughly to prepare component II;

[0033] (4) Preparation of component III:

[0034] According to the components and weight proportions in step (1), the weighed melamine of component III is added into container C to obtain component III, and the weighed component III is added into component II, and stirred evenly for later use;

[0035] The ambient temperature is controlled at 19-22°C, component I is mixed with a mixture of component II and component III, and after being evenly stirred, the mixture is immediately poured into a foaming box for foaming and then sliced ​​to obtain a polyurethane ceiling material resistant to moisture and heat deformation. The performance index data are shown in Table 4.

[0036] [Examples 2 to 5]

[0037] Examples 2 to 5 are carried out according to the steps in Example 1, except that the reaction raw materials and raw material ratios in the foaming formula are different, as shown in Table 2; the performance index data of the obtained polyurethane ceiling material are shown in Table 4.

[0038] Table 2 Weight parts of each component in the foaming formula of polyurethane ceiling material in Examples 1 to 5

[0039]

[0040]

[0041] [Comparative Examples 1 to 4]

[0042] (1) Prepare the raw materials according to the weight proportions of the components in Table 3;

[0043] (2) Preparation of component I: according to the weight proportion of component I in step (1), add the weighed components into container A in sequence, stir for 15 seconds, the material temperature is 20° C., and mix thoroughly;

[0044] (3) Controlling the ambient temperature to 20°C, quickly mixing and stirring component I and component II, and immediately pouring them into a foaming box for foaming after stirring evenly, to obtain a polyurethane ceiling material. The performance index data are shown in Table 4.

[0045] Table 3 Weight parts of each component in the foaming formula of polyurethane ceiling material in Comparative Examples 1 to 4

[0046]

[0047] Table 4 Performance test data of polyurethane ceiling materials of Examples 1 to 5 and Comparative Examples 1 to 4

[0048]

[0049]

[0050] Note: The test conditions for dimensional stability are 120℃, 100% RH (humidity) for 5 hours, 70℃ drying for 3 hours, and this cycle is repeated 3 times.

[0051] The present invention adopts full water foaming in the foaming formula, and uses melamine containing rigid groups in the formula, which can improve the support and dimensional stability of the PU sheet on the one hand, and reduce the deformation under high temperature and high humidity conditions. On the other hand, it can give the material excellent flame retardant properties. Second, the balance of gel and foaming is cleverly matched in the formula, which greatly gives the polyurethane foam the material characteristics of high open porosity. Avoid shrinkage or expansion caused by large changes in the external environment of the foam due to closed cells, and further improve the dimensional stability of the PU sheet. The dimensional stability, open porosity and flame retardancy of the polyurethane foam finally obtained are greatly improved. It can be seen from the performance data in Table 4 that the polyurethane foams prepared in Examples 1 to 5 are much higher in dimensional stability, open porosity and flame retardancy than Comparative Examples 1 to 4 under the same density conditions, and their compressive strength and tensile strength are also improved; the density of Example 4 is 34kg / m 3 , compression strength up to 235KPa, tensile strength up to 240Kpa, open porosity up to 92%, oxygen index of 20.6, and dimensional change rate of heat and humidity aging is (-1.8%)*1.4%*1.1%. It can be seen that the heat and humidity deformation resistant polyurethane ceiling material prepared by the present invention has the advantages of high open porosity, low dimensional change rate of heat and humidity aging, good flame retardant performance, and other physical properties have not decreased, and a good technical effect has been achieved, which can be used in the industrial application of polyurethane ceiling materials.

Claims

1. A polyurethane ceiling material resistant to moisture and heat deformation, comprising component I, component II and component III, wherein the weight ratio of component I: component II: component III is 100:100-200:5-15; in, In parts by weight, component I is composed of the following components: polyether polyol I: 30-40 parts, polyether polyol II: 20-30 parts, polyether polyol III: 30-40 parts, chain extender: 2-6 parts, foam stabilizer: 0.5-2.0 parts, catalyst: 0.2-0.7 parts, water: 2-4.5 parts; component II: isocyanate 100-200 parts; component III: melamine 5-15 parts; wherein the polyether polyol I uses glycerol as the initiator, and the grafting Propylene oxide, and then end-capped with ethylene oxide, the end-capping amount is 10% to 25%, and the hydroxyl value is 20 to 40 mgKOH / g; the polyether polyol II is formed by ring-opening polymerization with propylene oxide under the action of a catalyst using one of ethylene glycol, propylene glycol or diethylene glycol as an initiator, and the hydroxyl value is 215 to 350 mgKOH / g; the polyether polyol III is formed by polymerization of propylene oxide using glycerol as an initiator, and the hydroxyl value is 400 to 540 mgKOH / g; The foam stabilizer is selected from at least one of L580, B8409, HC605, HC580, B8540 and DC193; the catalyst is an amine catalyst, and the isocyanate in component II is selected from one of MDI, TDI and PAPI; the amine catalyst is selected from at least one of A33, A1, NE300, ZF10 and LE-710; the chain extender is selected from at least one of ethylene glycol, propylene glycol, butanediol, glycerol, hexylene glycol, diethylene glycol and dipropylene glycol; the isocyanate is selected from at least one of PM-200, M20S and M50; the component II is obtained by adding 100 to 200 parts of isocyanate into container B and stirring evenly, and the material temperature is 19 to 22°C; the component III is 5 to 15 parts of melamine, and the weighed melamine of component III is added into container C to obtain component III, and the weighed component III is added into component II and stirred evenly for later use.

2. A method for preparing the polyurethane ceiling material resistant to moisture and heat deformation according to claim 1, The following steps are involved: (1) Prepare component I by weight: polyether polyol I: 30-40 parts, polyether polyol II: 20-30 parts, polyether polyol III: 30-40 parts, chain extender: 2-6 parts, foam stabilizer: 0.5-2.0 parts, catalyst: 0.2-0.7 parts, water: 2-4.5 parts; component II: isocyanate 100-200 parts; component III: melamine 5-15 parts; wherein the polyether polyol I is initiator glycerol, grafted with propylene oxide, and then capped with ethylene oxide, the capping amount is 10%-25%, and the hydroxyl value is 20-40 mgKOH / g; the polyether polyol II is ethylene glycol, propylene glycol or diethylene glycol One of the components is an initiator, which is formed by ring-opening polymerization with propylene oxide under the action of a catalyst, and has a hydroxyl value of 215-350 mgKOH / g; the polyether polyol III is formed by polymerization of propylene oxide with propylene glycol as an initiator, and has a hydroxyl value of 400-540 mgKOH / g; the foam stabilizer is selected from at least one of L580, B8409, HC605, HC580, B8540 or DC193; the catalyst is an amine catalyst; the isocyanate in component II is selected from at least one of MDI, TDI or PAPI; the weight ratio of component I: component II: component III is 100:100-200:5-15; (2) Preparation of component I: According to the components and weight proportions in step (1), weighed polyether polyol I, polyether polyol II, polyether polyol III, foam stabilizer, catalyst, chain extender and water are added to container A in sequence, stirred for 10 to 20 seconds, the material temperature is 19 to 22° C., and mixed thoroughly; (3) Preparation of component II: According to the components and weight proportions in step (1), the weighed isocyanate of component II is added into container B and stirred evenly. The material temperature is 19-22° C. to prepare component II; (4) according to the components and weight proportions in step (1), the weighed melamine of component III is added into container C to obtain component III; (5) Add the weighed component III to component II and stir evenly for later use; (6) Controlling the ambient temperature to be 19-22° C., mixing component I with a mixture of component II and component III, and immediately pouring the mixture into a foaming box for foaming and slicing after uniform mixing, thereby obtaining a polyurethane ceiling material resistant to moisture and heat deformation.