Regenerated fiberboard and method for preparing the same using waste fiberboard

After removing the veneer and metal parts, the waste fiberboard is cooked and hot-pressed in sodium chlorite solution, which solves the problems of high energy consumption of crushing and waste of glue application, and improves the utilization rate of waste fiberboard and the integration of recycled fiberboard. performance.

CN116252372BActive Publication Date: 2024-11-26BEIJING FORESTRY UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310117966.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-11-26
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

In the prior art, the process of recycling waste fiberboards and reprocessing and manufacturing recycled fiberboards has problems such as high energy consumption for crushing, poor performance of recycled fibers, waste and low utilization rate.

Method used

The veneer and metal parts of the dismantled fiberboard were used to immerse the whole in sodium chlorite solution and evaporate and cook. The wood fibers were activated by acidic environment and the urea-formaldehyde resin were cured, and the recycled fiberboard was obtained without crushing and secondary glue.

Benefits of technology

Improve the utilization rate of waste fiberboard, reduce energy consumption and waste of secondary glue application, and prepare recycled fiberboard with excellent performance, with static curve strength ≧27Mpa, elastic modulus ≧2700Mpa, internal bond strength ≧0.6Mpa, water absorption and expansion Rate ≦45%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a regenerated fiberboard and a method for preparing the regenerated fiberboard using waste fiberboard. The preparation method comprises the following steps: 1) removing the veneer, edge banding and metal parts of the waste fiberboard; 2) immersing the waste fiberboard as a whole in a sodium chlorite solution for steaming; 3) cleaning the suspension on the surface of the waste fiberboard, drying, hot pressing, cooling, and obtaining a blank board; 4) sawing the edge of the blank board, sanding, and obtaining the regenerated fiberboard. The technical problem to be solved by the present invention is how to use the recycled waste fiberboard to manufacture the regenerated fiberboard, so that it does not need to crush the waste fiberboard to consume energy, nor does it need to waste by secondary sizing, and can maximize the use of the waste fiberboard to improve the utilization rate of the waste fiberboard. At the same time, the regenerated fiberboard prepared by the present invention has good comprehensive performance, and can meet the requirements of GB / T 11718 "Medium Density Fiberboard" with static bending strength ≥ 27Mpa, elastic modulus ≥ 2700Mpa, internal bonding strength ≥ 0.6Mpa, and water absorption thickness expansion rate ≤ 45%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycling waste fiberboards, and in particular relates to a regenerated fiberboard and a method for preparing the regenerated fiberboard by using the waste fiberboard. Background Art

[0002] my country produces a large amount of waste fiberboard and its products every year. Fully recycling waste fiberboard can save a lot of wood raw materials, effectively avoid environmental pollution and resource waste, and create considerable economic value. Fiberboard is a kind of artificial board made of separated wood fibers or fiber bundles as basic units, mixed with adhesives and waterproofing agents, and then formed under high temperature and high pressure.

[0003] In the prior art, the process of using recycled waste fiberboard to reprocess and manufacture regenerated fiberboard is similar to the raw material processing process during normal fiberboard production: generally, the waste fiberboard is first crushed, and then hydrothermal treatment, steam explosion or acid-base treatment is used to remove a large amount of adhesive originally used for wood fiber gluing in the fiberboard, and the wood fiber is regenerated and separated, and then the regenerated and separated wood fiber is glued and mixed with fresh wood fiber to prepare fiberboard.

[0004] The above-mentioned production process of manufacturing regenerated fiberboard using recycled waste fiberboard includes both a re-crushing process and a secondary gluing process. Therefore, there are problems such as high crushing energy consumption, poor performance of regenerated fibers, waste of secondary gluing, and low utilization rate of waste fiberboard. Summary of the invention

[0005] The main purpose of the present invention is to provide a regenerated fiberboard and a method for preparing the regenerated fiberboard using waste fiberboard. The technical problem to be solved is how to use the recycled waste fiberboard to manufacture the regenerated fiberboard so that it does not need to consume energy by crushing the waste fiberboard, nor does it need to waste by secondary gluing. It can also maximize the use of the waste fiberboard and improve the utilization rate of the waste fiberboard. At the same time, the regenerated fiberboard prepared by the present invention has good comprehensive performance, its static bending strength is ≧27Mpa, elastic modulus is ≧2700Mpa, internal bonding strength is ≧0.6Mpa, and water absorption thickness expansion rate is ≦45%, so it is more suitable for practical use.

[0006] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. According to the method proposed in the present invention, a method for preparing a recycled fiberboard using waste fiberboard comprises the following steps:

[0007] 1) Remove the veneer, edge banding and metal parts of the waste fiberboard;

[0008] 2) immersing the entire waste fiberboard in a sodium chlorite solution for steaming;

[0009] 3) cleaning the suspension on the surface of the waste fiberboard, drying, hot pressing, and cooling to obtain a blank plate;

[0010] 4) sawing the edges of the rough board and sanding it to obtain a regenerated fiberboard.

[0011] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0012] Preferably, in the aforementioned method, the waste fiberboard comprises cured urea-formaldehyde resin.

[0013] Preferably, in the aforementioned method, the mass concentration of the sodium chlorite solution is 1%.

[0014] Preferably, in the aforementioned method, the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20-50.

[0015] Preferably, in the aforementioned method, during the cooking, glacial acetic acid is used to adjust the pH value of the sodium chlorite solution to 4-5.

[0016] Preferably, in the aforementioned preparation method, the cooking temperature is 60-80° C. and the cooking time is 1-3 hours.

[0017] Preferably, in the aforementioned method, the air-drying is to place the waste fiberboard under ventilation conditions until it stops dripping.

[0018] Preferably, in the aforementioned method, the process conditions of hot pressing are as follows: the hot pressing temperature is 140° C., the hot pressing time is 300 to 420 seconds, and the hot pressing pressure is 2 to 3 MPa.

[0019] Preferably, in the aforementioned method, the mass concentration of the sodium chlorite solution is 1%; the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20-50; glacial acetic acid is used to adjust the pH value of the sodium chlorite solution to 4-5 during cooking; the cooking temperature is 60-80°C, and the cooking time is 1-3h; the process conditions of the hot pressing are as follows: the hot pressing temperature is 140°C, the hot pressing time is 300-420s, and the hot pressing pressure is 2-3Mpa.

[0020] The purpose of the present invention and the technical problems solved by the present invention are also achieved by the following technical solutions. A regenerated fiberboard proposed by the present invention is prepared according to the aforementioned method for preparing a regenerated fiberboard using waste fiberboard; its static bending strength is ≥27Mpa, elastic modulus is ≥2700Mpa, internal bonding strength is ≥0.6Mpa, and water absorption thickness expansion rate is ≤45%.

[0021] By means of the above technical solution, the regenerated fiberboard and the method for preparing the regenerated fiberboard using waste fiberboard proposed by the present invention have at least the following advantages:

[0022] The present invention provides a regenerated fiberboard and a method for preparing the regenerated fiberboard using waste fiberboard. The waste fiberboard is used as a raw material, and there is no need to crush the waste fiberboard or add adhesive for a second time. The regenerated fiberboard with good performance and stable quality can be obtained by only using acidic sodium chlorite activation and regeneration technology. The veneer, edge banding and metal parts on the waste fiberboard need only be removed, and then the whole waste fiberboard is completely immersed in a sodium chlorite solution for steaming. The two main components of the waste fiberboard, namely the solidified urea-formaldehyde resin and wood fiber that are present as adhesives in the original waste fiberboard, are made to regenerate adhesive substances through steaming. It is speculated that the reason may be that the wood fiber in the waste fiberboard may be oxidized and degraded by acidic sodium chlorite, thereby generating more active groups, which is conducive to bonding. On the other hand, the urea-formaldehyde resin originally used as an adhesive in the waste fiberboard is hydrolyzed in an acidic environment, and the obtained hydrolyzate is also conducive to bonding. Therefore, in the preparation process of the present invention, there is no need for secondary sizing, and the adhesive substance obtained by regeneration and activation with sodium chlorite can achieve bonding. Then , and then through the hot pressing method, the activated components are re-glued to obtain a regenerated fiberboard; the technical solution of the present invention can reduce the energy consumption and secondary gluing cost waste and environmental pollution in the prior art in the process of regenerating waste fiberboards, and at the same time can maximize the use of waste fiberboards. After the technical solution is promoted and applied in artificial board enterprises, it can greatly improve the utilization rate of waste fiberboards; and the comprehensive performance of the regenerated fiberboard prepared by the technical solution of the present invention is good; when the mass concentration of the sodium chlorite solution is 1% The mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20-50, glacial acetic acid is used to adjust the pH value of the sodium chlorite solution to 4-5 during cooking, the cooking temperature is 60-80°C, the cooking time is 1-3h, the hot pressing temperature is 140°C, the hot pressing time is 300-420s, and the hot pressing pressure is 2-3Mpa. The recycled fiberboard prepared under the process conditions has a static bending strength of ≧27Mpa, an elastic modulus of ≧2700Mpa, an internal bonding strength of ≧0.6Mpa, and a water absorption thickness expansion rate of ≦45%.

[0023] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION

[0024] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the specific implementation method, structure, characteristics and effects of a regenerated fiberboard and a method for preparing a regenerated fiberboard using waste fiberboard proposed by the present invention are described in detail below in combination with preferred embodiments.

[0025] The present invention provides a method for preparing a regenerated fiberboard using waste fiberboard, which comprises the following steps:

[0026] First, the veneer, edge banding, metal parts and other accessory parts of the waste fiberboard are removed, and impurities such as stones on the waste fiberboard are removed to prevent the veneer, edge banding, metal parts and stones and other impurities unrelated to the fiberboard itself from affecting the subsequent regeneration process and product quality of the regenerated fiberboard. The removal method can be carried out in any manner commonly used in the art, and the present invention is not specifically limited.

[0027] The second step is to immerse the waste fiberboard after removing the attached parts in a sodium chlorite solution for steaming. This step is one of the key steps of the technical solution of the present invention.

[0028] The specific operation is to put the sodium chlorite solution in a constant temperature water bath, and then completely immerse the waste fiberboard in the sodium chlorite solution for steaming to regenerate and activate it.

[0029] In order to allow the sodium chlorite solution to fully act on the various components in the waste fiberboard so as to better activate the wood fibers in the waste fiberboard, the technical solution of the present invention limits the mass concentration of the sodium chlorite solution to 0.8-1.2% on the one hand, and limits the mass ratio of the waste fiberboard to the sodium chlorite solution to 1:10-60 on the other hand; the regenerated fiberboards prepared under the process conditions can meet the national standard quality requirements for artificial boards.

[0030] In order to further improve the performance requirements of artificial boards, through a large number of experimental studies, the present invention preferably has a mass concentration of 1% of the sodium chlorite solution, and a mass ratio of the waste fiberboard to the sodium chlorite solution of 1:20-50; the mechanical properties of the regenerated fiberboard prepared under the process conditions can be greatly improved, and at this time its static bending strength is ≧33Mpa, the elastic modulus is ≧2900Mpa, and the internal bonding strength is ≧0.8Mpa; further, the present invention preferably has a mass concentration of 1% of the sodium chlorite solution, and a mass ratio of the waste fiberboard to the sodium chlorite solution of 1:50; the mechanical properties of the regenerated fiberboard prepared under the process conditions can be further improved, and at this time its static bending strength is ≧33Mpa, the elastic modulus is ≧3500Mpa, and the internal bonding strength is ≧1.7Mpa.

[0031] Furthermore, in order to better activate the components in the waste fiberboard, the present invention preferably includes cured urea-formaldehyde resin in the waste fiberboard, that is, the waste fiberboard previously used urea-formaldehyde resin as adhesive. The reason why the sodium chlorite can effectively reprocess the regenerated fiberboard is presumably that the sodium chlorite can activate the wood fiber and urea-formaldehyde resin components in the waste fiberboard; on the one hand, the wood fiber in the waste fiberboard may be oxidized and degraded by the acidic sodium chlorite, thereby generating more active groups, which is beneficial to adhesion; on the other hand, the urea-formaldehyde resin originally used as an adhesive in the waste fiberboard will also be hydrolyzed in an acidic environment, and the hydrolysis product obtained by the reaction is also beneficial to adhesion.

[0032] In order to obtain a better activation effect, the present invention preferably controls the pH value of the water bath solution to 4-5 during cooking to ensure that sodium chlorite can stably undergo chemical reactions under this environment, which is manifested in that it can continuously generate chlorine dioxide gas. The control of the pH value is preferably achieved by dripping glacial acetic acid into the cooking solution during the cooking process.

[0033] Furthermore, in order to obtain a better activation effect and balance the mechanical properties of the recycled fiberboard, the present invention preferably controls the cooking time to 1 to 3 hours during cooking. The reason is that if the cooking time is too short, the activation reaction may not be sufficient, affecting the adhesive effect in the hot pressing stage; and if the cooking time is too long, the loose strength of the fiberboard will be very poor, affecting its mechanical properties.

[0034] At the same time, in order to obtain a better activation effect and balance the mechanical properties of the recycled fiberboard, the present invention preferably controls the temperature of the water bath solution to 60-80°C during cooking. The reason is that if the temperature of the constant temperature water bath is set too low, the reaction between the fiberboard and sodium chlorite is insufficient due to the reaction temperature, thereby affecting the adhesive effect in the hot pressing stage; and if the temperature of the constant temperature water bath is set too high, the fiberboard is prone to deformation, making the fibers loose and the water content too high, which ultimately leads to poor comprehensive performance of the recycled fiberboard.

[0035] When the waste fiberboard is cooked, the cooking time and the cooking temperature have an interactive relationship. When the cooking temperature is low, in order to fully activate the waste fiberboard, it is preferred to cook for a longer time; the preferred cooking temperature of the present invention is 60°C and the cooking time is 3h; the regenerated fiberboard prepared under this process condition has excellent mechanical properties, at which time its static bending strength is ≧33Mpa, elastic modulus is ≧3500Mpa, and internal bonding strength is ≧1.7Mpa. When the cooking temperature is high, in order to avoid the waste fiberboard being over-activated, causing the wood fibers therein to become loose and deformed, and causing the water content in the waste fiberboard to be too high, it is preferred to cook for a shorter time; the preferred cooking temperature of the present invention is 80°C and the cooking time is 1h; the regenerated fiberboard prepared under this process condition has excellent mechanical properties, at which time its static bending strength is ≧35Mpa, elastic modulus is ≧2900Mpa, and internal bonding strength is ≧0.8Mpa.

[0036] The third step is to clean the suspension on the surface of the waste fiberboard, dry it, heat press it, and cool it to obtain a blank plate.

[0037] After the cooking is finished, the complete fiberboard is taken out from the constant temperature water bath, and then the waste fiberboard is rinsed with clean water to remove the sodium chlorite remaining on the surface of the fiberboard to prevent it from further acting on the waste fiberboard, so that its performance is in a stable state. Then, the fiberboard is placed in a ventilated environment for drying until the fiberboard does not drip water before entering the next process. Then, the activated components are re-glued by hot pressing to obtain a blank board.

[0038] In order to ensure the mechanical properties of the recycled fiberboard, the hot pressing process conditions are generally controlled at a hot pressing temperature of 120-140° C., a hot pressing time of 300-420 seconds, and a hot pressing pressure of 2-3 MPa.

[0039] When the hot pressing temperature is low, it may be difficult to melt the activated adhesive, resulting in its inability to fully exert its gluing effect, while when the hot pressing temperature is high, the mechanical properties of the wood fiber will be affected; the preferred hot pressing temperature of the present invention is 120-140°C; the hot pressing temperature is further preferably 140°C.

[0040] Both hot pressing time and hot pressing pressure will affect the performance of artificial boards. Under the same hot pressing temperature, when the hot pressing time is short and the hot pressing pressure is low, it may be difficult for the activated adhesive to fully function, thus affecting the secondary bonding between the wood fibers in the waste fiberboard; while when the hot pressing time is long and the hot pressing pressure is high, it is more conducive to the bonding of the fiberboard; at the same time, the degree of activation of the waste fiberboard by the sodium chlorite solution will also have a greater impact on the performance of the artificial board; the three factors are interrelated and influence each other, and when a better balance is reached, they can show better comprehensive performance.

[0041] When the waste fiberboard is activated by sodium chlorite solution with a mass concentration of 1%, when the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:50, the hot pressing temperature is 140°C, the hot pressing pressure is 2Mpa, and the hot pressing time is 300s, the comprehensive performance of the artificial board obtained under the process conditions is excellent, and its static bending strength is ≥33Mpa, the elastic modulus is ≥3500Mpa, and the internal bonding strength is ≥1.7Mpa. When the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20, the hot pressing temperature is 140°C, the hot pressing pressure is 3Mpa, and the hot pressing time is 420s, the comprehensive performance of the artificial board obtained under the process conditions is excellent, and its static bending strength is ≥35Mpa, the elastic modulus is ≥2900Mpa, and the internal bonding strength is ≥0.8Mpa.

[0042] Finally, the rough board is sawed and sanded to obtain the recycled fiberboard.

[0043] In the technical solution of the present invention, since the raw material is waste fiberboard that has not undergone any crushing treatment, there is no need for chipping, hot grinding and other processes for wood fiber separation. Therefore, the process is simple to operate, the process conditions are easy to meet, and the equipment is not complicated. It is also beneficial to saving wood resources and improving the utilization rate of waste fiberboard.

[0044] The present invention also proposes a regenerated fiberboard, which is prepared according to the above-mentioned method for preparing the regenerated fiberboard using the waste fiberboard. The mass concentration of the sodium chlorite solution is 1%; the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20-50; the pH value of the sodium chlorite solution is adjusted to 4-5 by using glacial acetic acid during cooking; the cooking temperature is 60-80°C, and the cooking time is 1-3h; the process conditions of the hot pressing are as follows: the hot pressing temperature is 140°C, the hot pressing time is 300-420s, and the hot pressing pressure is 2-3Mpa. The regenerated fiberboard prepared under the process conditions has a static bending strength of ≧27Mpa, an elastic modulus of ≧2700Mpa, an internal bonding strength of ≧0.6Mpa, and a water absorption thickness expansion rate of ≦45%.

[0045] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.

[0046] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.

[0047] Embodiment 1:

[0048] In this embodiment, a regenerated fiberboard is prepared from waste fiberboard, and the specific steps are as follows:

[0049] 1) Remove the veneer, edge banding and metal connectors, nails, stones and other impurities from the waste fiberboard.

[0050] 2) Completely immersing a waste fiberboard having a size of 300 mm × 300 mm × 3 mm and a weight of 202.5 g in a constant temperature water bath containing 10.125 kg of sodium chlorite solution for cooking; the mass concentration of the sodium chlorite solution is 1%; the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:50; adding glacial acetic acid dropwise to the sodium chlorite solution to adjust its pH value to 4-5; setting the temperature of the constant temperature water bath to 60° C., and the cooking time is 3 h.

[0051] 3) After the cooking is completed, the complete fiberboard is taken out and then cleaned with clean water to remove the sodium chlorite solution remaining on the surface; the fiberboard is then placed in a ventilated environment to dry until no water drips.

[0052] 4) The dried fiberboard is placed in a hot press for hot pressing at a temperature of 140° C., a time of 300 s, and a pressure of 2 MPa to obtain a rough version.

[0053] 5) The rough board is cooled, and then sawed and sanded to obtain a regenerated fiberboard.

[0054] The performance of the recycled fiberboard described in this embodiment was tested with reference to the national standard GB / T 17657-2013, and the test results are shown in Table 1 below.

[0055] It can be seen from the test results that the mechanical properties of the recycled fiberboard prepared in this embodiment are good and can meet the requirements of the national standard GB / T 11718 "Medium Density Fiberboard".

[0056] Table 1

[0057] Example 1 GB / T 11718-2021 Static bending strength MPa 33.51 27 Elastic modulus MPa 3505 2700 Internal bonding strength MPa 1.76 0.6 Water absorption thickness expansion rate % 32 45%

[0058] Embodiment 2:

[0059] In this embodiment, a regenerated fiberboard is prepared from waste fiberboard, and the specific steps are as follows:

[0060] 1) Remove the veneer, edge banding and metal connectors, nails, stones and other impurities from the waste fiberboard.

[0061] 2) Completely immersing a waste fiberboard having a size of 300 mm × 300 mm × 3 mm and a weight of 202.5 g in a constant temperature water bath filled with 4.05 kg of sodium chlorite solution for steaming; the mass concentration of the sodium chlorite solution is 1%; the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20; dropping glacial acetic acid into the sodium chlorite solution to adjust its pH value to 4-5; setting the temperature of the constant temperature water bath to 80° C., and the steaming time is 1 h.

[0062] 3) After the cooking is completed, the complete fiberboard is taken out and then cleaned with clean water to remove the sodium chlorite solution remaining on the surface; the fiberboard is then placed in a ventilated environment to dry until no water drips.

[0063] 4) The dried fiberboard is placed in a hot press for hot pressing at a temperature of 140° C., a time of 420 s, and a pressure of 3 MPa to obtain a rough version.

[0064] 5) The rough board is cooled, and then sawed and sanded to obtain a regenerated fiberboard.

[0065] The performance of the recycled fiberboard described in this embodiment was tested with reference to the national standard GB / T 17657-2013, and the test results are shown in Table 2 below.

[0066] It can be seen from the test results that the mechanical properties of the recycled fiberboard prepared in this embodiment are good and can meet the requirements of the national standard GB / T 11718 "Medium Density Fiberboard".

[0067] Table 2

[0068] Example 3 GB / T 11718-2021 Static bending strength MPa 35 27 Elastic modulus MPa 2900 2700 Internal bonding strength MPa 0.8 0.6 Water absorption thickness expansion rate % 30 45%

[0069] The technical features in the claims and / or the specification of the present invention may be combined, and the combination is not limited to the combination obtained by reference in the claims. The technical solution obtained by combining the technical features in the claims and / or the specification is also within the protection scope of the present invention.

[0070] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing regenerated fiberboard using waste fiberboard, characterized in that: It includes the following steps: 1) Remove the veneer, edge banding and metal parts of the waste fiberboard; 2) immersing the entire waste fiberboard in a sodium chlorite solution for steaming; the waste fiberboard includes a cured urea-formaldehyde resin; the steaming temperature is 60-80° C., the steaming time is 1-3 hours; the mass concentration of the sodium chlorite solution is 1%; the mass ratio of the waste fiberboard to the sodium chlorite solution is 1:20-50; during the steaming, glacial acetic acid is used to adjust the pH value of the sodium chlorite solution to 4-5; 3) cleaning the suspension on the surface of the waste fiberboard, drying, hot pressing, and cooling to obtain a blank board; the hot pressing temperature of the hot pressing is 120-140° C., the hot pressing time is 300-420 seconds, and the hot pressing pressure is 2-3 MPa; 4) sawing the edges of the rough board and sanding it to obtain a recycled fiberboard.

2. The method according to claim 1, characterized in that The air-drying step is to place the waste fiberboard under ventilation until no water drips.

3. The method according to claim 1, characterized in that The process conditions of the hot pressing are as follows: the hot pressing temperature is 140°C.

4. A regenerated fiberboard, characterized in that: It is prepared according to the method for preparing regenerated fiberboard using waste fiberboard according to any one of claims 1 to 3; Its static bending strength is ≧27Mpa, elastic modulus is ≧2700Mpa, internal bonding strength is ≧0.6Mpa, and water absorption thickness expansion rate is ≦45%.