A rapid solidification method for dredged soil from river excavation with high water content

By employing chemical pretreatment, mechanical pressure filtration, and inorganic gel stabilization methods, the solidification problem of dredged soil with high water content was solved, achieving rapid solidification and resource conservation. This provides a new engineering filler and reduces environmental pollution risks and costs.

CN116253495BActive Publication Date: 2024-11-12CHINA FIRST HIGHWAY ENGINEERING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211630156.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-12
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Existing technologies are ineffective in treating dredged soil with high moisture content, making it unsuitable for direct use in engineering construction. Furthermore, traditional solidification methods suffer from high costs, environmental pollution risks, and long solidification cycles.

Method used

A chemical pretreatment, mechanical pressure filtration, and inorganic gel stabilization method is adopted. Stabilized soil is formed by flocculation sedimentation, mechanical pressure filtration, and the addition of alkali-stimulated gel, and then rapidly solidified using materials such as steel slag powder, mineral powder, quicklime, and sodium silicate.

Benefits of technology

It achieves efficient solidification of dredged soil with high moisture content, reduces solidification time and cost, provides a new source of engineering filler, reduces environmental pollution risks, and has significant socio-economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116253495B_ABST
    Figure CN116253495B_ABST
Patent Text Reader

Abstract

The present invention discloses a rapid solidification method for high-water content river excavation dredged soil. The rapid solidification method is to form a high-performance regenerated engineering filler after chemical pretreatment, mechanical filter pressing dehydration, and inorganic gel stabilization of the high-water content dredged soil, and then use it in engineering construction. Among them, the chemical pretreatment adopts a mixed solution of 1-2wt% polysulfate ferric aluminum chloride and 1-3wt‰ amphoteric polyacrylamide in a mass ratio of 2:1 for flocculation; then an automatic slag filter is used to dehydrate and intercept the mud to form a semi-solid or solid mud cake; finally, alkali is used to stimulate gel stabilization, and after sufficient mixing, the final stable soil is formed through engineering filling and maintenance. The rapid solidification method of the present invention can make the soil strength of high-water content river excavation dredged soil reach more than 100kPa within 24 hours, with significant solidification effect, resource economy, and high environmental friendliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention mainly relates to the technical field of solidification and recycling of engineering abandoned soil, and in particular to a method for quickly solidifying dredged soil from river excavation with high water content. Technical Background

[0002] Dredging and desilting existing waterways in rivers, lakes and seas usually produces a large amount of high-water content mud, namely dredged soil. Due to its high water content, high compressibility and low bearing capacity, it cannot be directly used for engineering construction. At the same time, even for dredged soil with relatively low water content, the commonly used methods of soft soil solidification such as storage drying, chemical stabilization (cement, lime (lime + fly ash) and other inorganic materials stabilization), biological solidification and other methods for regeneration treatment also have defects such as large dosage, high cost, and finished product shrinkage and temperature shrinkage. In addition, industrial products such as cement and quicklime are high-energy consumption and high-carbon emission products, which are not conducive to resource conservation and environmental friendliness. Therefore, in practice, dredged soil can only be mainly stored and disposed of, which not only occupies a large amount of land, but also has a long consolidation period and environmental pollution risks. Finding new resource and environmentally friendly solidification methods to achieve large-scale engineering recycling of high-water content dredged soil has become the direction of new technology development in the field of dredging engineering. How to effectively reduce the solidification time and amount of solidifying agent of dredged soil while meeting the performance requirements of the project is the key to saving project costs and reducing environmental pollution risks.

[0003] However, so far, the relevant results are very limited. The new high-strength dredged soil curing agent disclosed in application number 201811300758.1 comprises: 6-12 parts by weight of cement, 8-14 parts by weight of mineral powder, 0.05-0.1 parts by weight of adhesive, 0.02-0.1 parts by weight of additive, 0.05-0.1 parts by weight of silane coupling agent, 0.1-0.15 parts by weight of terminal hydroxyl liquid polybutadiene, 0.1-0.15 parts by weight of diethylaminoethanol, and 0.01-0.05 parts by weight of fiber balls. The soft soil solidification enhancer disclosed in the application number 201610367011.2 is composed of 20%-30% lime, 65%-80% cement, and 1%-12.5% ​​enhanced activation stimulant, wherein the enhanced activation stimulant is composed of 97% lignin, 1.75% sodium lignin sulfonate, 0.45%-0.95% sodium sulfate, 1.5%-3% acrylamide, 12%-15.5% sodium silicate pentahydrate, and 70%-73% sodium metasilicate pentahydrate. The main agent of the above patents is cement, which is not conducive to resource conservation and energy conservation and carbon reduction. The modified material for improving the strength of soft soil foundation disclosed in application number 202111480388.6 includes 65-85 parts by weight of soft soil, 13-14.2 parts by weight of fly ash, 10.4-12.4 parts by weight of alkaline activator solution, and 0.1-0.3 parts by weight of xanthan gum modifier, but the limitation of this patent is that excessive alkalinity can easily lead to alkalinization of the soil and cause environmental pollution problems; the high-water content mud solidification method disclosed in application number 202110846500.7 refers to flocculation treatment and solidification treatment of high-water content mud in sequence, but the limitation of this patent is that the industrial materials used are of many types and high cost; the high-efficiency solidification method for high-water content soft soil site disclosed in application number 201910160700.X refers to first pre-loading and drainage according to vacuum pre-loading and other methods, and then secondary repair and reinforcement through high-pressure grouting, but the limitation of this patent is that the pre-loading and dehydration effect is poor and the curing cycle is too long. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method for rapid solidification of dredged soil from river excavation with high water content, which solves the current problems of storage of dredged soil from river excavation with high water content occupying land and being unable to be directly utilized. The method is suitable for the solidification of soft soil with high water content and on-site recycling of engineering projects, which can effectively save engineering costs, reduce environmental pollution, and has significant social and economic benefits.

[0005] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:

[0006] A rapid solidification method for dredged soil from river excavation with high water content, wherein the dredged soil with high water content is subjected to chemical pretreatment, mechanical filtration to achieve rapid dehydration, and inorganic gel stabilization to form a regenerated engineering filler with excellent performance, and finally stabilized soil is formed through maintenance.

[0007] As an improvement, the specific steps of the chemical pretreatment are: preparing a flocculation mixture with a mass ratio of 2:1 using 1-2wt% of polyaluminum ferric sulfate chloride and 1-3wt‰ of amphoteric polyacrylamide solution, adding 3-5wt% of the flocculation mixture into the high-water content dredged soil for chemical flocculation precipitation treatment, and obtaining an initial high-water content mud by fully stirring and letting it stand for 30-40 minutes.

[0008] As an improvement, the specific steps of the mechanical filter pressing dehydration are: using an automatic slag discharge filter to filter the initial high-water content mud to turn it into a semi-solid or solid mud cake with a water content of no more than 35% and a filtration accuracy range of 0.2-100μm.

[0009] As an improvement, the inorganic gel stabilization is to add alkali-induced gel accounting for 10-20wt% of high-water content dredged soil into the semi-solid or solid mud cake. The specific steps are: evenly spread 2-3cm thick curing agent on the mud cake storage site, deep plowing with the help of a tiller until the difference in curing agent dosage is very small after multi-point sampling, and no further plowing is required, thereby forming a filler that can be reused in engineering. Finally, it is used for engineering filling and formed into stabilized soil after maintenance.

[0010] A further improvement is that the alkali-induced gel is mixed with steel slag powder, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide powder, and the corresponding mass mixing ratios are 27-36wt%, 13-18wt%, 13-16wt%, 27-30wt% and 0.03-0.06‰, and the particle sizes of steel slag powder, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide powder are all less than 200 mesh.

[0011] A further improvement is that the curing temperature is 20±3° C. and the relative humidity is 95%.

[0012] Beneficial Effects

[0013] Compared with the prior art, the rapid solidification method of high-water-content river channel excavation dredged soil of the present invention has the following advantages:

[0014] (1) It can realize the high-value, green and low-carbon resource recycling of industrial solid waste (steel slag and slag);

[0015] (2) Avoid using cement, reduce costs, and reduce carbon emissions, which is beneficial to resource conservation and economic and environmental protection;

[0016] (3) Efficiently solidifying dredged soil with high water content can provide a new filler supply channel for the project. At the same time, it can also effectively shorten the solidification time of dredged soil with high water content and speed up the progress of project implementation;

[0017] (4) The implementation method is simple and feasible, saves land, can effectively save project costs, reduce environmental pollution, and has significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A flowchart of a rapid solidification method for dredged soil from a river excavation with a high water content;

[0019] Figure 2 The time required for different flocculants to complete flocculation and sedimentation treatment;

[0020] Figure 3 Strength changes of solidified soil at different temperatures. Specific implementation plan

[0021] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0022] Implementation steps include:

[0023] 1. Prepare a flocculation mixture with a mass ratio of 2:1 and a concentration of 1-2wt% using polyaluminum ferric sulfate chloride and amphoteric polyacrylamide, and add it to the high-water-content dredged soil at a ratio of 3-5wt% to carry out chemical flocculation precipitation treatment, and obtain an initial high-water-content mud by fully stirring and standing for 30-40 minutes;

[0024] 2. Use an automatic slag filter to filter the initial high-water content mud to turn it into a semi-solid or solid mud cake with a water content of no more than 35%. The filtration accuracy range is 0.2-100μm;

[0025] 3. Use steel slag powder, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide to prepare alkali-stimulated gel, and evenly spread it on the surface of semi-solid or solid mud cake in the storage site, and use a tiller to deep-turn until the difference in curing agent dosage is very small after multi-point sampling, and then do not turn it over again, so as to form filler that can be reused in engineering;

[0026] 4. The dredged soil recycled fill material is used for engineering filling and maintained to a specified age to form stable soil.

[0027] Example 1

[0028] Firstly, the high-water content dredged soil was subjected to flocculation and sedimentation treatment. 500g of the high-water content dredged soil was taken, and polyaluminum ferric sulfate chloride, amphoteric polyacrylamide, polyaluminum ferric sulfate chloride and amphoteric polyacrylamide (mass ratio of 2:1) were used to prepare flocculation liquids with a concentration of 2wt%, and the flocculation liquids were added into the high-water content dredged soil at a ratio of 3-5wt% to carry out chemical flocculation and sedimentation treatment. After being fully stirred and allowed to stand, the time required for the formation of the initial high-water content mud was observed, and the test was carried out according to the scheme in Table 1.

[0029] Table 1 Flocculation sedimentation test plan and results

[0030]

[0031] Figure 2 The results of the flocculation and sedimentation time of different flocculants can be seen from the figure that when the same flocculant concentration and dosage are used to treat the same amount of dredged soil with high water content, the flocculation time required by the flocculation mixture of polyaluminum ferric chloride sulfate and amphoteric polyacrylamide is the shortest.

[0032] Therefore, the best flocculation and precipitation treatment effect is achieved by using polyaluminum ferric chloride sulfate and amphoteric polyacrylamide (mass ratio is 2:1) to prepare a flocculation solution with a concentration of 2wt%.

[0033] Take 500kg of high-water content mud after coagulation and precipitation treatment, and use an automatic slag filter to mechanically press and dehydrate it. As the filtration time increases, more and more solid impurities are trapped on the filter screen, which makes the filter cake thickness increase, the filtration resistance increase, and the pressure in the tank increase. When the pressure rises to a certain value, it is necessary to discharge slag, stop inputting the filtrate into the tank, and then pass steam to dry the filter cake. Generally, the filter cake thickness is controlled at 2-3 cm, and a semi-solid or solid mud cake with a water content of no more than 35% can be obtained.

[0034] Engineering practice shows that, under normal circumstances, the cement (as a curing agent) content in cement soil is 7% to 15%.

[0035] To be conservative, the total amount of alkali-induced gel material in the dredged soil was fixed at 15% (relative to the mass of the dredged soil with high water content), and steel slag powder, mineral powder, quicklime, sodium silicate, and hydroxylated graphene oxide were set according to the scheme in Table 2. Dredged soil solidification cylindrical samples with different water contents were prepared, and 7d unconfined compressive strength tests were carried out.

[0036] The specific steps for preparing the high-water content dredged soil sample solidified by steel slag powder include:

[0037] Take the dredged soil after flocculation sedimentation and mechanical filter press dehydration treatment, and determine the amount of steel slag, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide under the corresponding working conditions according to the test plan. Mix the dredged soil, steel slag powder, mineral powder, quicklime and sodium silicate evenly, and put the hydroxylated graphene oxide into water to form a homogeneous solution. Then add the homogeneous solution to the mixture of dredged soil, steel slag and mineral powder, stir until it is a homogeneous slurry, load it into the saturator several times, and use vibration to exhaust and compact it; after curing for 24 hours at a temperature of 20±3℃ and a relative humidity of 95%, demould it, and place it in the same curing environment again to the specified age. The sample preparation is completed using a 39.1mm×80mm triaxial saturator, and the sample preparation is controlled to be formed within 20min, with at least 3 parallel samples for each working condition.

[0038] Temperature directly affects the development of soil strength. In order to explore the influence of curing temperature on the strength of solidified dredged soil, the total dosage of alkali-activated gel in the fixed dredged soil was 15%, and the steel slag powder, mineral powder, quicklime and sodium silicate were set according to the scheme in Table 2. The cylindrical samples were prepared with the dosage of hydroxylated graphene oxide being 0.05‰, and a 7d unconfined compressive strength test was carried out.

[0039] Table 2 Temperature test plan

[0040]

[0041] During the test, an electronic universal testing machine was used to perform axial loading at a constant rate of 1 mm / min until the specimen was damaged. The test was manually stopped and the test data was saved.

[0042] The results are as follows Figure 3 As shown in the figure, it can be seen that the compressive strength of solidified dredged soil increases almost linearly with the increase of temperature. When the temperature is 20℃ and 40℃, its 7d uniaxial compressive strength has reached 158.24kPa and 299.49kPa, indicating that the temperature has a significant effect on the strength of high-water content dredged soil solidified by steel slag powder and mineral powder. Therefore, in order to shorten the hardening time of dredged soil, the temperature of dredged soil in engineering construction can be appropriately increased.

Claims

1. A method for rapid solidification of dredged soil from river excavation with high water content, characterized in that: The high-water content dredged soil is chemically pretreated, mechanically filtered and dehydrated, and then stabilized with inorganic gel to form a regenerated engineering filler with excellent performance, and finally stabilized soil is formed through maintenance; The specific steps of the chemical pretreatment are: preparing a flocculation mixture with a mass ratio of 2:1 using a 1-2wt% polysulfate aluminum ferric chloride and a 1-3wt‰ amphoteric polyacrylamide solution, adding 3-5wt% of the flocculation mixture to the high-water content dredged soil for chemical flocculation precipitation treatment, and obtaining an initial high-water content mud by fully stirring and standing for 30-40 minutes; The specific steps of the mechanical filter pressing dehydration are: using an automatic slag filter to filter the initial high-water content mud to make it into a semi-solid state or solid mud cake, the water content of which is not more than 35%, and the filtering accuracy range is 0.2-100μm; The inorganic gel stabilization is to add 10-20wt% of alkali-induced gel to the semi-solid or solid mud cake, and the specific steps are to first spread 2-3cm thick curing agent manually in the mud cake storage site, and then use a tiller to deep plow until the difference in curing agent dosage is very small after multi-point sampling, and then no more plowing is done, so as to form a filler that can be reused in engineering, and finally, it is used for engineering filling and formed into stabilized soil after curing; The alkali-induced gel is formed by mixing steel slag powder, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide powder, and the corresponding mass mixing ratios are 27-36wt%, 13-18wt%, 13-16wt%, 27-30wt% and 0.03-0.06‰, and the sum of the masses of each component is 100%; the particle sizes of the steel slag powder, mineral powder, quicklime, sodium silicate and hydroxylated graphene oxide powder are all less than 200 meshes.

2. The method for rapid solidification of dredged soil from river excavation with high water content according to claim 1, characterized in that: The curing temperature is 20±3° C. and the relative humidity is 95%.