A grinding aid, preparation method, use and grinding liquid containing the same
By combining electrostatic repulsion agents with nonionic polymer dispersants and solvents, and using a specific abrasive combination, the problems of low removal rate and scratches in silicon carbide substrate polishing slurries were solved, achieving efficient and easy-to-clean silicon carbide polishing results.
Patent Information
- Application Number
- CN202310109882.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-14
AI Technical Summary
Existing silicon carbide substrate polishing slurries suffer from problems such as low removal rate, high surface roughness after polishing, severe scratches, and difficulty in cleaning, making it difficult to meet the requirements of high precision and high efficiency polishing.
By employing the synergistic effect of multi-charge electrostatic repulsion agents and nonionic polymer dispersants, combined with amphiphilic water-soluble, hydrophilic and lipophilic solvents, and using large-size agglomerated diamond abrasives and small-size alumina abrasives, the dispersibility and suspension are improved and the surface roughness is reduced through chemomechanical action.
It achieves highly dispersed and efficient silicon carbide grinding, reduces the risk of scratches, is easy to clean, ensures surface uniformity and low roughness, and improves grinding rate and product yield.
Smart Images

Figure CN116254060B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to grinding liquid technology, and in particular to a grinding aid, a preparation method, a use and a grinding liquid containing the same. Background Art
[0002] Wide bandgap semiconductor materials represented by silicon carbide (SiC) and gallium nitride (GaN) are the third generation of semiconductors after silicon (Si) and gallium arsenide (GaAs). Compared with traditional semiconductor materials such as Si and GaAs, SiC has excellent properties such as high thermal conductivity, high breakdown field strength, high saturated electron drift velocity and high bonding energy, and has great application prospects in high temperature, high frequency, high power and radiation-resistant devices. Among them, the development of high-efficiency switching elements used in power supplies for engines driving electric bicycles, electric vehicles and hybrid vehicles has attracted much attention.
[0003] Since the hardness of silicon carbide is second only to diamond, diamond abrasives are generally used as grinding materials when precision grinding silicon carbide single crystal substrates. Diamond abrasives are expensive. In order to increase the removal rate of silicon carbide, the abrasive particle size must be increased, which inevitably causes scratches. At the same time, due to the presence of large diamond particles, the silicon carbide substrate is easily broken when the force is uneven, resulting in a decrease in product yield.
[0004] Silicon carbide substrates used in the semiconductor field must have high precision in terms of flatness, thickness difference (TTV), surface roughness (Ra), etc. In addition, the particle residues such as grinding debris generated by grinding must be easily cleaned. However, due to the extremely high hardness and excellent corrosion resistance of silicon carbide single crystals, the processability of silicon carbide substrates is poor, and it is difficult to maintain a high-quality surface at a high grinding speed. Some silicon carbide polishing fluids are disclosed in the prior art, such as:
[0005] CN114231251A discloses a diamond grinding liquid for rough grinding of silicon carbide wafers and its preparation method, belonging to the field of ultra-precision grinding processing technology. The grinding liquid is made of water and the following raw materials in parts by weight: 0.5-2 parts of diamond micropowder, 0.1-0.5 parts of surfactant, 0.2-0.8 parts of thickener, 0.5-7 parts of lubricant, 0.05-1 parts of dispersant, 1.5-5 parts of active agent for rust prevention and pH adjustment, and 0.01-0.2 parts of bactericide. The grinding liquid fully considers the cleaning performance and rust prevention performance of the grinding liquid.
[0006] CN114806502A discloses a grinding liquid for processing silicon carbide wafers and a preparation method thereof, wherein the grinding liquid comprises: 0.5-10 parts of diamond micropowder, 0.5-10 parts of dispersant, 1-20 parts of suspending agent and 50-98 parts of water. In the grinding liquid, the particle size of the diamond micropowder is concentrated, and the number of coarse particles is much smaller than that of the diamond grinding liquid prepared by the traditional method, thereby effectively preventing large particles of diamond from scratching the silicon carbide wafer.
[0007] As mentioned above, the prior art has disclosed a variety of polishing liquids (auxiliaries), but these polishing liquids (auxiliaries) have the following defects to varying degrees: low removal rate in the double-sided polishing process of SiC substrates, high surface roughness after polishing, severe scratches, and difficulty in cleaning. Therefore, the polishing liquids (auxiliaries) in the prior art currently have various defects and are difficult to meet the increasingly demanding polishing requirements. Therefore, it is urgent to develop a silicon carbide substrate polishing liquid with high dispersion, high efficiency, and easy cleaning for double-sided polishing of SiC wafers. Summary of the invention
[0008] The purpose of the present invention is to propose a grinding aid to solve the problems of low removal rate of existing grinding liquid, high surface roughness after grinding, serious scratches and difficulty in cleaning. The grinding liquid containing the grinding aid has the characteristics of high dispersion, high efficiency and easy cleaning. The abrasive can also be suspended and dispersed for a long time, has strong wetting and spreading ability, fast removal rate, low surface roughness of processed silicon carbide, and no obvious scratches. The grinding aid has excellent dispersing effect and can effectively disperse the nanoparticles generated in the grinding process to avoid adsorption on the abrasive surface, thereby significantly improving the life of the abrasive.
[0009] To achieve the above object, the technical solution adopted by the present invention is: a grinding aid, comprising the following components in weight proportions:
[0010]
[0011] Furthermore, the dispersant is a nonionic polymer dispersant.
[0012] Furthermore, the dispersant is one or more of polyacrylate, polyoxyethylene alcohol, polyether polyol and EO / PO block polymer.
[0013] Furthermore, the molecular weight of the polyacrylate is 2000-10000.
[0014] Furthermore, the molecular weight of the polyacrylate is preferably 2000-5000.
[0015] Furthermore, the molecular weight of the polyoxyethylene alcohol is 5000-10000.
[0016] Furthermore, the molecular weight of the polyoxyethylene alcohol is preferably 5000-8000.
[0017] Furthermore, the molecular weight of the polyether polyol is 1000-5000.
[0018] Furthermore, the molecular weight of the polyether polyol is preferably 2000-5000.
[0019] Furthermore, the molecular weight of the EO / PO block polymer is 2000-10000.
[0020] Furthermore, the molecular weight of the EO / PO block polymer is preferably 2000-5000.
[0021] Furthermore, the dispersant is preferably an EO / PO block polymer.
[0022] Furthermore, the dispersant is 1-5 parts.
[0023] Furthermore, the electrostatic repulsion agent is an organic metal salt containing a multi-charge structure.
[0024] Furthermore, the electrostatic repulsion agent is one or more of zinc 2-ethylhexanoate, zinc 4-hydroxybenzenesulfonate, zinc 4-methylbenzenesulfinate, zinc diethylphosphinate, zinc disodium ethylenediaminetetraacetate and chromium 2-ethylhexanoate.
[0025] Furthermore, the electrostatic repulsion agent is preferably zinc 2-ethylhexanoate.
[0026] Furthermore, the electrostatic repulsion agent is 0.5-1 part.
[0027] Furthermore, the weight ratio of the dispersant to the electrostatic repulsion agent is 30-1:1.
[0028] Furthermore, the weight ratio of the dispersant to the electrostatic repulsion agent is preferably 10-1:1.
[0029] Furthermore, the weight ratio of the dispersant to the electrostatic repulsion agent is most preferably 4:1.
[0030] The present invention adopts a multi-charged electrostatic repulsive agent and a non-ionic polymer dispersant in a coordinated manner. The long chain structure of the dispersant is entangled on the surface of agglomerated diamond abrasive particles, thereby increasing the steric hindrance between the particles and preventing the abrasive from agglomerating and settling. At the same time, the electrostatic repulsive agent has a strong electrostatic particle repulsion effect, can be effectively adsorbed on the abrasive surface, effectively inhibits the electrostatic adsorption of the abrasive, and exhibits a stronger electrostatic repulsion effect in the grinding liquid system, thereby preventing the abrasive or grinding chip particles that are broken during the grinding process from agglomerating or flocculating, thereby avoiding scratches on the silicon carbide substrate.
[0031] Furthermore, the amphiphilic solvent is one or more of diethylene glycol methyl ether, ethylene glycol ethyl ether acetate, triethylene glycol butyl ether, ethylene glycol ethyl ether, propylene glycol phenyl ether, tripropylene glycol methyl ether and glycerol acetone acetal.
[0032] Furthermore, the amphiphilic solvent is preferably triethylene glycol butyl ether.
[0033] Furthermore, the amphiphilic solvent is 30-40 parts.
[0034] Furthermore, the lipophilic solvent refers to a solvent with an HLB of 3-5.
[0035] Furthermore, the lipophilic solvent is one or more of n-propanol, n-butanol, isopropanol, tetrahydrofuran and methyl ethyl ketone.
[0036] Furthermore, the lipophilic solvent is preferably methyl ethyl ketone.
[0037] Furthermore, the lipophilic solvent is 5-10 parts.
[0038] Furthermore, the hydrophilic solvent refers to a solvent with an HLB of 7-10.
[0039] Furthermore, the hydrophilic solvent is one or more of dimethyl sulfoxide, N-pyrrolidone, N,N-dimethylacetamide, sulfolane and N,N-dimethylformamide.
[0040] Furthermore, the hydrophilic solvent is preferably dimethyl sulfoxide.
[0041] Furthermore, the hydrophilic solvent is 30-40 parts.
[0042] Furthermore, the weight ratio of the amphiphilic solvent, the lipophilic solvent and the hydrophilic solvent is 2-10:1:2-8.
[0043] Furthermore, the weight ratio of the amphiphilic solvent, the lipophilic solvent and the hydrophilic solvent is preferably 3-6:1:2-4.
[0044] Furthermore, the weight ratio of the amphiphilic solvent, the lipophilic solvent and the hydrophilic solvent is most preferably 3:1:3.
[0045] The grinding aid of the present invention adopts a technical scheme of compounding an amphiphilic aqueous solvent, a hydrophilic solvent and a lipophilic solvent, and is made into a uniform mixed solvent according to the principle of similar compatibility. The mixed solvent has a lower surface energy relative to the water solvent system and is easier to be washed clean by water. The lipophilic solvent has a stronger chemical reaction with the silicon crystal surface of silicon carbide, and the hydrophilic solvent has a stronger chemical reaction with the carbon crystal surface of silicon carbide. The use of hydrophilic and lipophilic solvents at the same time can keep the chemical reaction rate of each crystal surface of silicon carbide the same, and improve the uniformity of grinding; the Gemini surfactant with an amphiphilic structure has more hydrophilic and hydrophobic groups. Under the action of the lipophilic-hydrophilic solvent, the hydrophilic group and the lipophilic group are fully extended, so that a double-layer directional adsorption layer is formed on the surface of silicon carbide, which has a lower surface interface energy, reduces the surface tension of silicon carbide, and allows the abrasive to spread quickly on the surface of the grinding disc, ensuring that the force on silicon carbide is uniform, the surface roughness is low after grinding, and the thickness is uniform.
[0046] Furthermore, the wetting agent is a Gemini surfactant.
[0047] Furthermore, the wetting agent is one or more of polyoxyethylene ether quaternary ammonium salt, acetylene glycol polyoxyethylene ether, ethane-1,2-di(dodecyldimethylammonium chloride), ethane-1,2-di(tetradecyldimethylammonium chloride), butane-1,4-di(hexadecyldimethylammonium chloride), propane-1,3-di(lauric acid imidazoline), butane-1,4-di(myristic acid imidazoline), brominated gemini dodecyl 2-methylimidazole, gemini dodecyl benzimidazole and gemini dodecyl-2-methylbenzimidazole.
[0048] Furthermore, the wetting agent is preferably acetylene glycol polyoxyethylene ether.
[0049] Furthermore, the molecular weight of the polyoxyethylene ether quaternary ammonium salt is 1000-3000.
[0050] Furthermore, the molecular weight of the polyoxyethylene ether quaternary ammonium salt is preferably 1000-2000.
[0051] Furthermore, the molecular weight of the acetylene glycol polyoxyethylene ether is 800-2000.
[0052] Furthermore, the molecular weight of the acetylene glycol polyoxyethylene ether is preferably 800-1000.
[0053] Furthermore, the wetting agent is 0.5-0.8 parts.
[0054] Furthermore, the softening agent is one or more of sodium persulfate, sodium hypochlorite, sodium perchlorate, sodium chlorate, potassium iodate, potassium periodate and potassium ferrocyanide.
[0055] Furthermore, the softening agent is preferably potassium periodate.
[0056] Furthermore, the softener is 0.5-1 part.
[0057] Another object of the present invention is to disclose a method for preparing the above-mentioned grinding aid, comprising the following steps:
[0058] Step 1: Add an amphiphilic solvent, a hydrophilic solvent, a dispersant, a wetting agent and a lipophilic solvent into a stirred tank, stir and mix them evenly to obtain a clear and transparent solution;
[0059] Step 2: Add a softener and an electrostatic repulsion agent to the solution obtained in step 1 while stirring, and stir evenly to prepare a grinding aid.
[0060] Furthermore, the stirring time in step 1 is 30-60 min.
[0061] Furthermore, the stirring speed in step 2 is 50-100 r / min.
[0062] Furthermore, the stirring time in step 2 is 10-60 min.
[0063] Furthermore, the stirring time in step 2 is preferably 20-40 min.
[0064] Another object of the present invention is to disclose the use of the grinding aid in the field of grinding silicon carbide, gallium nitride, silicon nitride, aluminum nitride and sapphire substrates, and is particularly suitable for precision grinding of silicon carbide.
[0065] Another object of the present invention is to disclose a grinding liquid, comprising the above-mentioned grinding aid and abrasive.
[0066] Furthermore, the mass ratio of the grinding aid to the abrasive is 40-140:1.
[0067] Furthermore, the mass ratio of the grinding aid to the abrasive is preferably 60-80:1.
[0068] Furthermore, the abrasive is agglomerated diamond abrasive and / or small-sized abrasive.
[0069] Furthermore, the abrasive comprises the following components in weight proportion:
[0070] Agglomerated diamond abrasive 0.5-1 part;
[0071] Small size abrasive 0.1-1 part;
[0072] Furthermore, the agglomerated diamond abrasive is 0.8-1 part.
[0073] Furthermore, the small-size abrasive is 0.1-0.5 parts.
[0074] Furthermore, the agglomerated diamond abrasive has a particle size of 10-30 μm.
[0075] Furthermore, the agglomerated diamond abrasive particle size is preferably 10-20 μm.
[0076] Furthermore, the agglomerated diamond abrasive is formed by mixing and sintering 50-500nm aluminum oxide, 100-500nm silicon oxide and 200-1000nm diamond.
[0077] Furthermore, the agglomerated diamond abrasive is preferably formed by mixed sintering of 50-100nm aluminum oxide, 200-300nm silicon oxide and 200-500nm diamond.
[0078] Furthermore, the agglomerated diamond abrasive preparation method is as follows:
[0079] S1: First, weigh three abrasives according to the mass ratio of aluminum oxide: silicon oxide: diamond = 2:1:40-10, add them into a stirring kettle, then add isopropanol, and stir to form a uniform slurry;
[0080] S2: adding polyvinyl butyral resin, polyvinyl pyrrolidone, polyacrylate and sodium lauryl sulfate to the slurry obtained in S1, and stirring to prepare a mixed slurry;
[0081] S3: adding the mixed slurry obtained in S2 into a ball mill, and mixing by ball milling to obtain a mixed slurry;
[0082] S4: using a centrifugal spray dryer to spray granulate the slurry obtained in S3; passing the collected spherical powder through 400 mesh and 1000 mesh ultrasonic sieves to sieve out the intermediate agglomerated abrasive;
[0083] S5: drying the organic solvent in the agglomerated abrasive obtained in S4;
[0084] S6: placing the agglomerated abrasive obtained in S5 in a sintering furnace for vacuum sintering, and finally annealing in air to obtain agglomerated diamond abrasive.
[0085] Furthermore, the mass ratio of aluminum oxide: silicon oxide: diamond is preferably 2:1:10.
[0086] Furthermore, the mass ratio of the total mass of the three abrasives to isopropanol is 1:1-3.
[0087] Furthermore, the stirring time in S1 is 10-20 min.
[0088] Furthermore, the mass ratio of the slurry, polyvinyl butyral resin, polyvinyl pyrrolidone, polyacrylate and sodium lauryl sulfate in S2 is 2000:1-10:10-100:10-50:1-10.
[0089] Furthermore, the mass ratio of the slurry, polyvinyl butyral resin, polyvinyl pyrrolidone, polyacrylate and sodium lauryl sulfate in S2 is preferably 2000:5-10:10-50:10-30:1-5.
[0090] Furthermore, the molecular weight of the polyvinyl butyral resin in S2 is 10000-100000.
[0091] Furthermore, the molecular weight of the polyvinyl butyral resin in S2 is preferably 10,000-50,000.
[0092] Furthermore, the stirring speed in S2 is 50-100 r / min, and the stirring time is 30-60 min.
[0093] Furthermore, the ball milling speed in S3 is 50-200 r / min.
[0094] Furthermore, the ball milling speed in S3 is preferably 50-100 r / min.
[0095] Furthermore, the grinding balls and the grinding jar of the S3 ball mill are made of high-purity zirconium oxide.
[0096] Further, S3 slurry: ball mass ratio = 1:1-3.
[0097] Furthermore, the S3 ball milling mixing time is 10-60 min.
[0098] Furthermore, the S3 ball milling mixing time is preferably 10-30 min.
[0099] Furthermore, the S4 spray drying conditions were: hot air inlet temperature 80°C, outlet temperature 40°C, inlet air volume 4L / min, outlet air volume 4L / min, centrifugal atomizer speed 15000r / min, and slurry pumping rate 30mL / min.
[0100] Furthermore, the drying conditions in S5 are: drying temperature 50-70° C., and drying time 1-10 h.
[0101] Furthermore, the drying time in S5 is preferably 5-10 hours.
[0102] Furthermore, the vacuum sintering temperature in S6 is 1500-1800° C., and the sintering time is 6-8 hours.
[0103] Furthermore, the annealing temperature in air in S6 is 150-200° C., and the annealing time is 8-10 hours.
[0104] Furthermore, the small-sized abrasive is one or a mixture of α-phase aluminum oxide, zirconium oxide and silicon oxide.
[0105] Furthermore, the small-sized abrasive is preferably α-phase aluminum oxide.
[0106] Furthermore, the small-size abrasive grain size is 0.5-3 μm.
[0107] Furthermore, the small-sized abrasive particles preferably have a diameter of 0.5-1 μm.
[0108] The abrasive in the grinding liquid of the present invention is compounded with large-sized agglomerated diamond abrasive, small-sized aluminum oxide mixed abrasive and softener. The self-sharpening property of high-hardness diamond particles on the surface of the large-sized agglomerated diamond abrasive can improve the grinding rate and avoid deep scratches caused by simple large-sized single crystal or polycrystalline diamond abrasive. The presence of the softener can form soft oxides with low hardness on the surface of silicon carbide, cooperate with the small-sized abrasive with low hardness, repair the scratches generated by the large-sized agglomerated diamond abrasive through chemical mechanical action, and reduce the surface roughness of the silicon carbide after grinding.
[0109] Another object of the present invention is to disclose a method for preparing a grinding liquid, comprising the following steps:
[0110] Under stirring conditions, agglomerated diamond abrasives and small-sized abrasives are added to the grinding aid, and stirred to form a uniform suspended mixed liquid to prepare a grinding liquid.
[0111] Furthermore, the stirring speed is 50-100 r / min.
[0112] Furthermore, the stirring speed is preferably 50-80 r / min.
[0113] Furthermore, the stirring time is 10-60 min.
[0114] Furthermore, the stirring time is preferably 30-60 min.
[0115] Another object of the present invention is to disclose a use of a grinding liquid in the field of grinding silicon carbide, gallium nitride, silicon nitride, aluminum nitride and sapphire substrates, and is particularly suitable for precision grinding of silicon carbide.
[0116] Grinding of substrates such as silicon carbide, gallium nitride, silicon nitride, aluminum nitride, sapphire, etc., especially for precision grinding of silicon carbide.
[0117] Further, the silicon carbide is ground with a grinding liquid, including the following grinding process:
[0118] Rotation speed: 30r / min; Pressure: 4.5kpa; Disk temperature: 25-35℃; Grinding time: 20min.
[0119] The grinding aid, preparation method, use and grinding liquid containing the same of the present invention have the following advantages compared with the prior art:
[0120] 1. The grinding aid of the present invention adopts a multi-charged electrostatic repulsion agent and a non-ionic polymer dispersant in a synergistic manner. The long chain structure of the dispersant is entangled on the surface of the agglomerated diamond abrasive particles, increasing the steric hindrance between the particles to prevent the agglomeration and sedimentation of the abrasive. At the same time, the electrostatic repulsion agent has a strong electrostatic particle repulsion effect, can be effectively adsorbed on the abrasive surface, effectively inhibiting the electrostatic adsorption of the abrasive, and showing a stronger electrostatic repulsion effect in the grinding liquid system, preventing the broken abrasive or grinding chip particles from agglomerating or flocculating during the grinding process, and avoiding scratches on the silicon carbide substrate.
[0121] 2. The grinding aid of the present invention adopts a technical solution of compounding an amphiphilic aqueous solvent, a hydrophilic solvent and a lipophilic solvent. According to the principle of like-is-compatible, a uniform mixed solvent is prepared. The mixed solvent has a lower surface energy relative to the aqueous solvent system and is easier to be washed clean by water. The lipophilic solvent has a stronger chemical reaction with the silicon crystal surface of silicon carbide, and the hydrophilic solvent has a stronger chemical reaction with the carbon crystal surface of silicon carbide. The use of hydrophilic and lipophilic solvents at the same time can keep the chemical reaction rate of each crystal surface of silicon carbide the same, and improve the uniformity of grinding; the Gemini surfactant with an amphiphilic structure has more hydrophilic and hydrophobic groups. Under the action of the lipophilic-hydrophilic solvent, the hydrophilic group and the lipophilic group are fully extended, which promotes the formation of a double-layer directional adsorption layer on the surface of silicon carbide, has a lower surface interface energy, reduces the surface tension of silicon carbide, and allows the abrasive to spread quickly on the surface of the grinding disc, ensuring that the force on silicon carbide is uniform, the surface roughness is low after grinding, and the thickness is uniform.
[0122] 3. The abrasive of the grinding liquid of the present invention is a compound of large-sized agglomerated diamond abrasive, small-sized aluminum oxide mixed abrasive and softener. The self-sharpening property of the high-hardness diamond particles on the surface of the large-sized agglomerated diamond abrasive can improve the grinding rate and avoid deep scratches caused by simple large-sized single crystal or polycrystalline diamond abrasive. The presence of the softener can form a low-hardness soft oxide on the surface of silicon carbide, which cooperates with the low-hardness small-sized abrasive to repair the scratches caused by the large-sized agglomerated diamond abrasive through chemical mechanical action, thereby reducing the surface roughness of the silicon carbide after grinding.
[0123] Therefore, the grinding aid and grinding liquid of the present invention have very good application prospects and large-scale industrial promotion potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0124] Figure 1Schematic diagram of the surface after grinding in Example 13 (a), magnified 100 times;
[0125] Figure 2 Schematic diagram of the surface microscope after grinding of Comparative Example 1 (a), magnified 100 times;
[0126] Figure 3 Schematic diagram of the surface after grinding in Example 13 (II), magnified 100 times;
[0127] Figure 4 Schematic diagram of the surface microscope after grinding of Comparative Example 1 (II), magnified 100 times;
[0128] Figure 5 The suspension performance comparison between the examples and comparative examples is shown in Figure 13 on the left and comparative example 1 on the right. DETAILED DESCRIPTION
[0129] The present invention is further described below in conjunction with embodiments:
[0130] Examples 1-12
[0131] Examples 1-12 disclose a variety of grinding aids, the compositions and weight ratios of which are shown in Table 1, and the preparation methods thereof are as follows:
[0132] Step 1: Add an amphiphilic solvent, a hydrophilic solvent, a dispersant, a wetting agent and a lipophilic solvent into a stirred tank, stir for 30 minutes to mix evenly, and obtain a clear and transparent solution;
[0133] Step 2: Add a softener and an electrostatic repulsion agent to the solution obtained in step 1 under stirring at 100 r / min, and stir for 60 minutes to form a uniform clear liquid.
[0134] Table 1 Components and weight ratios of grinding aids in Examples 1-12
[0135]
[0136]
[0137] The grinding aids described in Examples 1-12 have a density of 1.05-1.15 g / mL and a pH value of 7-9.
[0138] Examples 13-24
[0139] Examples 13-24 disclose a variety of polishing liquids, whose compositions and weight ratios are shown in Table 1, and their preparation methods are as follows:
[0140] Step 1: Add an amphiphilic solvent, a hydrophilic solvent, a dispersant, a wetting agent and a lipophilic solvent into a stirred tank, stir for 60 minutes to mix evenly, and obtain a clear and transparent solution;
[0141] Step 2: Add softener and electrostatic repulsion agent to the solution obtained in step 1 under stirring at 80 r / min, and stir for 30 minutes until a uniform clear liquid is formed.
[0142] Step 3: Under the stirring condition of 50 r / min, add agglomerated diamond abrasive and small-sized abrasive to the solution obtained in step 2, and stir for 50 minutes until the mixture is uniformly mixed to form a uniform suspension mixture, thereby preparing a grinding liquid.
[0143] Table 2 Composition and weight ratio of the grinding liquid of Examples 13-24
[0144]
[0145]
[0146] Comparative Examples 1-9
[0147] Comparative Examples 1-9 disclose a variety of grinding liquids, the components and weight ratios of which are shown in Table 3, and the preparation methods are the same as those of Example 13.
[0148] Table 3 Components and weight ratios of the grinding fluids of Comparative Examples 1-9
[0149]
[0150]
[0151] The preparation method of agglomerated diamond abrasive used in Examples 13-24 and Comparative Examples 1-9 is as follows:
[0152] Step 1: First, weigh 1 kg of three abrasives according to the ratio of 50 nm aluminum oxide: 200 nm silicon oxide: 200 nm diamond = 2:1:10, add them into a stirring kettle, add 1 kg of isopropanol, and stir for 20 minutes to make a uniform slurry.
[0153] Step 2: Add 5 g of polyvinyl butyral resin, 50 g of polyvinyl pyrrolidone, 10 g of polymethyl acrylate, and 5 g of sodium dodecyl sulfate to the above slurry, and stir at 80 r / min for 30 min to prepare a mixed slurry.
[0154] Step 3: Add the above slurry into a ball mill, set the ball mill speed to 100r / min, select high-purity zirconia materials for the grinding balls and the ball mill jar, the slurry: ball mass ratio = 1:1, and mix for 30 minutes to obtain a mixed slurry.
[0155] Step 4: The obtained slurry was spray granulated using a centrifugal spray dryer. The spray drying conditions were: hot air inlet temperature 80°C, outlet temperature 40°C, inlet air volume 4L / min, outlet air volume 4L / min, centrifugal atomizer speed 15000r / min, slurry pumping rate 30mL / min, and the collected spherical powder was passed through 400 mesh and 1000 mesh ultrasonic sieves to sieve out the intermediate abrasive.
[0156] Step 5: Dry the agglomerated abrasive obtained above in an oven at 50° C. for 10 hours to dry the organic solvent on the agglomerated diamond abrasive.
[0157] Step 6: Place the above-mentioned agglomerated abrasive in a sintering furnace, sinter at 1800° C. in vacuum for 8 hours, and finally anneal in air at 1200° C. for 10 hours to obtain agglomerated diamond abrasive.
[0158] Performance Testing
[0159] Next, various properties of the above-mentioned polishing fluids were tested, as follows.
[0160] Table 4 shows the performance test data of Examples 13-24 and Comparative Examples 1-9. It can be seen that the polishing liquid of the examples has good suspension, fast polishing rate and good surface quality after polishing.
[0161] Table 4 Performance test data of Examples 13-24 and Comparative Examples 1-9
[0162]
[0163] in:
[0164] The polishing liquids prepared in the above Examples 13-24 and Comparative Examples 1-9 were subjected to polishing tests using a 4-inch silicon carbide substrate to test removal rate, TTV, Ra, maximum scratch width after polishing, surface contamination, and suspension.
[0165] Surface dirt test after grinding: After grinding, take out the silicon carbide wafer, rinse it with deionized water for 1 minute, blow it dry, and observe whether there is any grinding debris or particles left on the surface under an optical microscope. If there is no residue, it is excellent, and if there is residue, it is poor.
[0166] Surface dirt test after cleaning: Use a cleaning agent to perform two stages of ultrasonic cleaning at 80°C for 10 minutes, then use deionized water to perform ultrasonic cleaning at 80°C. After drying, observe the surface under an optical microscope to see if there are any grinding chips or other residues. If there are no residues, it is excellent; if there are residues, it is poor.
[0167] Maximum scratch width test after grinding: The cleaned silicon carbide substrate was tested for maximum scratch width under a microscope at the same magnification and field of view, and the average value was taken after three measurements.
[0168] Suspension test: After continuous high-speed shear stirring at 500r / min for 8h, the silicon carbide grinding fluid was left to stand for 1h to observe the abrasive suspension.
[0169] Grinding process:
[0170] Grinding equipment: double-sided grinding machine;
[0171] Silicon carbide wafer size: 4 inches;
[0172] Number of test pieces: 240 pieces;
[0173] Speed: 30r / min;
[0174] Pressure: 4.5kpa;
[0175] Plate temperature: 25-35℃;
[0176] Grinding time: 20min.
[0177] Figure 1 The surface of Example 13 after grinding was magnified 100 times by a microscope, and the surface was clean without obvious dirt particles; Figure 2 The surface of the comparative example 1 after grinding was magnified 100 times by a microscope, and there were obvious dirt particles on the surface; Figure 3 The surface of Example 13 after grinding was magnified 100 times by microscope, and there was no scratch and the surface was uniform; Figure 4 The surface of the comparative example 1 was magnified 100 times by a microscope after grinding, and there were multiple scratches on the surface to verify the scratches; Figure 5 The suspension performance comparison between the examples and the comparative examples. The left side shows that Example 13 is completely suspended without stratification, and the abrasive is distributed in the entire grinding liquid system. The right side shows that the abrasive is precipitated in Comparative Example 1 without suspension performance.
[0178] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A grinding aid, characterized in that: The composition includes the following components in weight ratio: Dispersant 1-10 parts; 0.1-1 part of electrostatic repulsion agent; 30-50 parts of amphiphilic solvent; 5-20 parts of lipophilic solvent; 20-40 parts of hydrophilic solvent; Wetting agent 0.5-1 part; Softener 0.1-1 part; The dispersant is one or more of polyacrylate, polyoxyethylene alcohol, polyether polyol and EO / PO block polymer; The electrostatic repulsion agent is one or more of zinc 2-ethylhexanoate, zinc 4-hydroxybenzenesulfonate, zinc 4-methylbenzenesulfinate, zinc diethylphosphinate, zinc disodium ethylenediaminetetraacetate and chromium 2-ethylhexanoate.
2. The grinding aid according to claim 1, characterized in that: The amphiphilic solvent is one or more of diethylene glycol methyl ether, ethylene glycol ethyl ether acetate, triethylene glycol butyl ether, ethylene glycol ethyl ether, propylene glycol phenyl ether, tripropylene glycol methyl ether and glycerol acetone acetal; And / or, the lipophilic solvent refers to a solvent with an HLB of 3-5; And / or, the hydrophilic solvent refers to a solvent with an HLB of 7-10.
3. The grinding aid according to claim 1, characterized in that: The wetting agent is a Gemini surfactant.
4. The grinding aid according to claim 1, characterized in that: The softening agent is one or more of sodium persulfate, sodium hypochlorite, sodium perchlorate, sodium chlorate, potassium iodate, potassium periodate and potassium ferrocyanide.
5. A method for preparing the grinding aid according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Add an amphiphilic solvent, a hydrophilic solvent, a dispersant, a wetting agent and a lipophilic solvent into a stirred tank, stir and mix them evenly to obtain a clear and transparent solution; Step 2: Add a softener and an electrostatic repulsion agent to the solution obtained in step 1 while stirring, and stir evenly to prepare a grinding aid.
6. Use of the grinding aid according to any one of claims 1 to 4 in the field of grinding silicon carbide, gallium nitride, silicon nitride, aluminum nitride and sapphire substrates.
7. A polishing liquid, characterized in that: The invention comprises the grinding aid and abrasive according to any one of claims 1 to 4.
8. The polishing liquid according to claim 7, characterized in that: The abrasive is agglomerated diamond abrasive and / or small-sized abrasive, and the small-sized abrasive is one or a mixture of α-phase aluminum oxide, zirconium oxide and silicon oxide.
9. Use of the grinding liquid according to claim 7 in the field of grinding silicon carbide, gallium nitride, silicon nitride, aluminum nitride and sapphire substrates.