A weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material and a preparation method thereof
By modifying carbon black into an esterified carbon black masterbatch and dispersed and curing in a silane crosslinked polyethylene insulating material, the problem of difficulty in dispersing carbon black in insulating material is solved, and the mechanical and electrical properties of the material are improved, satisfying the satisfaction of The weather resistance and trace resistance of outdoor cables are required.
Patent Information
- Application Number
- CN202211427473.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-15
AI Technical Summary
When existing insulating materials are added with high content of carbon black, it is difficult to ensure uniform dispersion of carbon black, affecting mechanical strength and electrical strength, resulting in mechanical cracking and breakdown of cables, and it is difficult to meet the weather resistance and trace resistance requirements of outdoor overhead wires and cables. .
By modifying the carbon black into an esterified carbon black masterbatch and dispersing and curing in a silane cross-linked polyethylene insulating material, the uniform distribution and fixation of the carbon black is ensured, and the weather resistance and trace resistance of the material are improved.
It realizes uniform dispersion and curing of high-content carbon black, improves the mechanical strength, electrical strength and weathering and trace resistance of the insulating material, and adapts to the application needs of harsh outdoor environments.
Smart Images

Figure BDA0003943468810000021 
Figure BDA0003943468810000022 
Figure BDA0003943468810000171
Abstract
Description
Technical Field
[0001] The invention relates to the field of insulating materials, and in particular to a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material and a preparation method thereof. Background Art
[0002] In recent years, with the continuous development of social economy, the demand for outdoor overhead wires and cables has been increasing, and the amount of wires and cables used has been doubling. Wire and cable insulation materials need to have high volume resistivity, low dielectric loss, good heat aging resistance and other characteristics to adapt to outdoor applications.
[0003] Outdoor overhead insulated cables usually work in harsh environments. They are prone to photo-oxidation aging under long-term climatic conditions such as air, rain, and light. At the same time, cables will generate higher temperatures when transmitting high voltages and large currents. The increase in temperature will affect the electrical insulation of the material, causing creepage and tracking of the cable insulation layer, which will lead to cable breakdown. These multiple factors require that the insulation materials of wires and cables also have good weather resistance and tracking resistance.
[0004] In order to meet the above performance requirements, the industry uses carbon black to modify cross-linked polyethylene to achieve weather resistance and electrical tracking resistance. However, in the actual material system, carbon black is added to the polymer matrix in the form of particles. It is difficult to disperse well when the addition amount is more than 2%, and it is difficult to ensure the uniform dispersion of carbon black, which affects the mechanical and electrical strength of the insulation layer itself, and brings risks of mechanical cracking and breakdown to the cable.
[0005] The Chinese patent application publication number CN114163716 A discloses a high carbon black light-oxidation-resistant silane cross-linked polyethylene insulation material and a preparation method. The disclosed insulation material preparation raw materials are made of linear low-density polyethylene resin A, linear low-density polyethylene resin B, high-pressure low-density polyethylene, silane coupling agent, initiator, antioxidant, light stabilizer, carbon black, organic-inorganic composite modifier, surfactant, compatibilizer, catalyst, and rheology modifier. However, it is difficult to ensure the uniform dispersion of carbon black in the material in actual production, thereby affecting the performance of wires and cables and causing quality defects.
[0006] Therefore, there is an urgent need for an insulating material with high carbon black and uniform carbon black distribution to ensure the weather resistance and tracking resistance of the insulating material to adapt to the application of overhead wires and cables in outdoor environments. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a weather-resistant and electric-tracking-resistant silane cross-linked polyethylene insulating material and a preparation method thereof. The insulating material provided by the present invention uses silane cross-linked overhead polyethylene as a matrix, has the characteristics of high volume resistivity and low dielectric loss, and adds a high content of carbon black to make it have good weather resistance and electric-tracking resistance; the present invention further improves the weather resistance and electric-tracking resistance of the insulating material by preparing carbon black into esterified carbon black masterbatch, and provides a preparation method of esterified carbon black masterbatch and a preparation method of the insulating material.
[0008] The specific technical scheme of the present invention is:
[0009] On the one hand, the present invention provides a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulation material, including material A and material B;
[0010] Material A includes the following components in parts by weight:
[0011]
[0012] Material B includes the following components in parts by weight:
[0013]
[0014] In the weather-resistant and tracking-resistant silane cross-linked polyethylene insulating material provided by the present invention, silane cross-linked overhead polyethylene is used as the matrix, and has the characteristics of high volume resistivity and low dielectric loss, and by adding carbon black with a content of more than 3%, a material with good weather resistance and tracking resistance is obtained. Carbon black is added to the polymer matrix in the form of particles, and it is difficult to disperse well in the case of a large addition amount, and it is difficult to ensure the uniformity of carbon black, which causes the material to be prone to mechanical cracking and breakdown. Therefore, the present invention modifies the carbon black, adds it to the material in the form of an esterified carbon black masterbatch, improves the compatibility of the resin matrix in the carbon black particle state to change the high self-polymerization property of the carbon black itself, and obtains a polyethylene insulating material with a high content of carbon black and uniform dispersion of carbon black. Specifically, the principle of uniformly dispersing carbon black in the insulating material of the present invention is as follows: the insulating material is divided into material A and material B, and the carbon black is modified into an esterified carbon black masterbatch that can be grafted and compatible with the vinyl body at the molecular microscopic level. 30-40 parts of the esterified carbon black masterbatch are initially dispersed in the B material, and then when the A material and the B material are mixed, the esterified carbon black masterbatch is solidified while the polyethylene matrix is cross-linked and copolymerized under the action of the silane coupling agent, and finally is uniformly dispersed and fixedly present in the insulating material.
[0015] Furthermore, adding 5-15 parts of polypropylene resin to material A can improve the strength and heat resistance of polyethylene.
[0016] Preferably, the mass ratio of material A to material B in the insulating material is 90-95:5-10.
[0017] Specifically, the preparation method of esterified carbon black masterbatch comprises the following steps:
[0018] S1: Add 30-37 wt% formaldehyde solution to carbon black, add NaOH to adjust the pH to 7.0-9.2, and react at 60° C. for 3-4 hours to obtain hydroxymethylated carbon black.
[0019] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 to 3 hours to obtain a reaction base liquid. Add hydroxymethylated carbon black to the reaction base liquid, react at 70 to 80°C for 4 to 6 hours, and dry and grind to obtain esterified carbon black masterbatch.
[0020] In the preparation process of esterified carbon black masterbatch, the surface of carbon black is first hydroxymethylated, and then maleic anhydride is ring-opened and grafted on the surface of carbon black molecules under the catalytic action of perchloric acid in DMSO to obtain esterified carbon black. When preparing esterified carbon black, if maleic anhydride is directly grafted with carbon black molecules, the grafting rate is extremely low due to the existence of interface barriers, and the surface contact performance of carbon black and maleic anhydride in DMSO must be improved first. In order to improve the surface contact performance, one is to first hydroxymethylate the surface of carbon black and improve it by using the affinity of hydroxyl and anhydride groups, and the other is to activate maleic anhydride by ultrasonication for 2 to 3 hours under the action of perchloric acid, which is in a preparatory state for the formation of carbon cation ring opening. In the final grafting reaction, maleic anhydride opens the ring while carbon cations bond to hydroxyl groups.
[0021] Specifically, in step S1, the mass volume ratio of carbon black to formaldehyde solution is 7kg:7-7.3L.
[0022] Specifically, the molar volume ratio of maleic anhydride, perchloric acid and DMSO in the reaction base liquid of step S2 is 0.5-1 mol: 0.4-0.6 mol: 1 L. The mass volume ratio of hydroxymethylated carbon black to the reaction base liquid is 0.8-1 kg: 1 L.
[0023] Specifically, the melt index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melt index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melt index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0024] Preferably, the silane coupling agent is one or more of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl tri(β-methoxyethoxy)silane.
[0025] Preferably, the initiator is diisopropylbenzene peroxide, the dehydrating agent is trimethoxymethane, and the catalyst is dibutyltin dilaurate.
[0026] Preferably, the antioxidant is one or more of antioxidant 300, antioxidant 1076, antioxidant 1010, antioxidant AT 10, antioxidant DSTP and antioxidant DLTP.
[0027] On the other hand, the present invention provides a method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material, comprising the following steps:
[0028] (1) Preparation of material A:
[0029] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0030] ② Mix and evenly stir the silane coupling agent, dehydrating agent, initiator and antioxidant, dissolve them, add them into the mixed material, extrude and mix them through a twin-screw extruder to obtain a mixed initial material;
[0031] ③After adding esterified carbon black masterbatch, granulate and dry through single screw extruder;
[0032] (2) Preparation of material B:
[0033] ① Dry polyethylene resin 1, polyethylene resin 2 and esterified carbon black masterbatch, add silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst to mix, extrude, infiltrate, granulate and dry;
[0034] (3) Cross-linking and plasticization:
[0035] ① Material A and material B are mixed, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking to obtain the insulating material.
[0036] The insulating material includes material A and material B. After carbon black is modified into esterified carbon black masterbatch, it can be grafted compatible with vinyl at the molecular microscopic level. 30-40 parts of esterified carbon black masterbatch are initially dispersed in material B. Material A and material B are prepared separately and then mixed and formed. In the process of mixing material A and material B, material B is dispersed in material A, and the esterified carbon black masterbatch is further dispersed. Finally, under the action of silane coupling agent, the polyethylene matrix is cross-linked and copolymerized. At the same time, the esterified carbon black masterbatch is fixed and dispersed through the action of the ester group and carboxyl group on its molecule, and finally is evenly dispersed and fixedly present in the insulating material.
[0037] Specifically, in step (1), the temperature of each zone of the twin-screw extrusion mixing is: I 118-122°C, II 138-142°C, III 123-127°C, IV 178-182°C, V 193-197°C, VI 198-202°C, VII 198-202°C, VIII 198-202°C, IX 198-202°C, and the die head 188-192°C;
[0038] Specifically, in step (1), the temperature of each zone of the single screw extrusion granulation is: Ⅰ 143 ~ 147 ° C, Ⅱ 163 ~ 167 ° C, head 173 ~ 177 ° C.
[0039] Specifically, the temperatures of the extrusion zones in step (2) are: I 58-62°C, II 138-142°C, III 178-182°C, IV 148-152°C, V 188-192°C, VI 188-192°C, VII 188-192°C, VIII 188-192°C, IX 188-192°C, and the die is 178-182°C.
[0040] Preferably, the temperatures of the zones of the single screw extruder in step (3) are: Ⅰ 125°C, Ⅱ 145°C, Ⅲ 165°C, Ⅳ 185°C, Ⅴ 195°C, flange 195°C, neck 205°C, and head 215°C.
[0041] Preferably, the cross-linking temperature in step (3) is 90-95° C. and the time is 4-10 hours.
[0042] Compared with the prior art, the present invention has the following technical effects:
[0043] (1) The present invention provides an insulating material that can be added with a high content of carbon black of more than 3% and can maintain excellent mechanical strength and electrical strength.
[0044] (2) The present invention modifies carbon black and disperses and fixes it in two steps during the preparation process, so that high-content carbon black can be evenly dispersed and fixed in the insulating material provided by the present invention.
[0045] (3) The insulating material provided by the present invention has a smooth surface, large margins for thermal elongation and thermal shrinkage performance indicators, and excellent weather resistance and electrical tracking resistance. DETAILED DESCRIPTION
[0046] The present invention will be further described below in conjunction with the embodiments.
[0047] Example 1
[0048] Preparation of esterified carbon black masterbatch:
[0049] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0050] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0051] Preparation of weather-resistant and electric-track-resistant silane cross-linked polyethylene insulation material:
[0052] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0053] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0054] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0055] (1) Preparation of material A:
[0056] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0057] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0058] Table 1
[0059] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 120℃ 140℃ 125℃ 180℃ 195℃ 200℃ 200℃ 200℃ 200℃ 200℃
[0060] ③ After adding carbon black modified masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0061] Table 2
[0062] Ⅰ Ⅱ Machine head 145℃ 165℃ 175℃
[0063] (2) Preparation of material B:
[0064] ① Polyethylene resin 1, polyethylene resin 2 and carbon black modified masterbatch were dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst were added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0065] Table 3
[0066] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 60℃ 140℃ 180℃ 150℃ 190℃ 190℃ 190℃ 190℃ 190℃ 180℃
[0067] (3) Cross-linking and plasticization:
[0068] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0069] Table 4
[0070] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Flange Machine neck Machine head 125℃ 145℃ 165℃ 150℃ 195℃ 195℃ 205℃ 215℃
[0071] Example 2
[0072] Preparation of esterified carbon black masterbatch:
[0073] S1: Add 30 wt% formaldehyde solution to carbon black at a mass volume ratio of 1kg:1L, add NaOH to adjust the pH to 7.0, and react at 60°C for 3h to obtain hydroxymethylated carbon black.
[0074] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2.5 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.5 mol:0.4 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:0.8 kg, react at 70°C for 6 hours, dry and grind to obtain esterified carbon black masterbatch.
[0075] Preparation of weather-resistant and electric-track-resistant silane cross-linked polyethylene insulation material:
[0076] Raw materials of material A (parts by weight): 40 parts of polyethylene resin 1, 10 parts of polyethylene resin 2, 5 parts of polypropylene resin, 3 parts of esterified carbon black masterbatch, 1.5 parts of vinyl triethoxysilane, 0.13 parts of diisopropylbenzene peroxide, 0.12 parts of trimethoxymethane, and 0.04 parts of antioxidant 300.
[0077] Raw materials for material B (parts by weight): 20 parts of polyethylene resin 1, 20 parts of polyethylene resin 2, 3 parts of silicone powder, 0.5 parts of dibutyltin dilaurate, 2 parts of antioxidant 1010, 30 parts of esterified carbon black masterbatch, 0.5 parts of anti-copper agent 905, 0.5 parts of phenyl o-hydroxybenzoate, and 0.5 parts of hindered amine light stabilizer.
[0078] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0079] (1) Preparation of material A:
[0080] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0081] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a preliminary mixed material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 5.
[0082] Table 5
[0083] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 118℃ 138℃ 123℃ 178℃ 193℃ 198℃ 198℃ 198℃ 198℃ 188℃
[0084] ③ After adding carbon black modified masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 6.
[0085] Table 6
[0086] Ⅰ Ⅱ Machine head 143℃ 163℃ 177℃
[0087] (2) Preparation of material B:
[0088] ① Polyethylene resin 1, polyethylene resin 2 and carbon black modified masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 7.
[0089] Table 7
[0090] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 58℃ 142℃ 182℃ 152℃ 192℃ 192℃ 192℃ 192℃ 192℃ 182℃
[0091] (3) Cross-linking and plasticization:
[0092] ① Material A and material B were mixed in a mass ratio of 95:8, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 92°C for 6 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 8.
[0093] Table 8
[0094] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Flange Machine neck Machine head 125℃ 145℃ 165℃ 150℃ 195℃ 195℃ 205℃ 215℃
[0095] Example 3
[0096] Preparation of esterified carbon black masterbatch:
[0097] S1: Add 35 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.3L, add NaOH to adjust the pH to 9.2, and react at 60°C for 3-4h to obtain hydroxymethylated carbon black.
[0098] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 3 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 1 mol:0.5 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:0.9 kg, react at 80°C for 4 hours, dry and grind to obtain esterified carbon black masterbatch.
[0099] Preparation of weather-resistant and electric-track-resistant silane cross-linked polyethylene insulation material:
[0100] Raw materials of material A (parts by weight): 60 parts of polyethylene resin 1, 20 parts of polyethylene resin 2, 15 parts of polypropylene resin, 8 parts of esterified carbon black masterbatch, 2 parts of vinyl tri(β-methoxyethoxy) silane, 0.23 parts of diisopropylbenzene peroxide, 0.21 parts of trimethoxymethane, and 0.11 parts of antioxidant 1076.
[0101] Raw materials of material B (parts by weight): 30 parts of polyethylene resin 1, 30 parts of polyethylene resin 2, 5 parts of silicone powder, 1 part of dibutyltin dilaurate, 4 parts of antioxidant, 40 parts of esterified carbon black masterbatch, 1 part of anti-copper agent 905, 1 part of phenyl o-hydroxybenzoate, and 1 part of hindered amine light stabilizer.
[0102] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0103] (1) Preparation of material A:
[0104] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0105] ② Mix and evenly stir the silane coupling agent, dehydrating agent, initiator and antioxidant, dissolve them, add them into the mixture, extrude and mix them through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 9.
[0106] Table 9
[0107] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 122℃ 142℃ 127℃ 182℃ 197℃ 202℃ 202℃ 202℃ 202℃ 192℃
[0108] ③ After adding carbon black modified masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 10.
[0109] Table 10
[0110] Ⅰ Ⅱ Machine head 147℃ 167℃ 173℃
[0111] (2) Preparation of material B:
[0112] ① Polyethylene resin 1, polyethylene resin 2 and carbon black modified masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 11.
[0113] Table 11
[0114] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Ⅵ Ⅶ Ⅷ Ⅸ Machine head 62℃ 138℃ 178℃ 148℃ 188℃ 188℃ 188℃ 188℃ 188℃ 178℃
[0115] (3) Cross-linking and plasticization:
[0116] ① Material A and material B were mixed in a mass ratio of 92:5, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 90°C for 10 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 12.
[0117] Table 12
[0118] Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ Flange Machine neck Machine head 125℃ 145℃ 165℃ 150℃ 195℃ 195℃ 205℃ 215℃
[0119] Comparative Example 1 (the main difference from Example 1 is that the esterified carbon black masterbatch is replaced by the ordinary carbon black masterbatch)
[0120] Insulation material preparation:
[0121] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0122] Raw materials of material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0123] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0124] (1) Preparation of material A:
[0125] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0126] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0127] ③ After adding carbon black masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0128] (2) Preparation of material B:
[0129] ① Polyethylene resin 1, polyethylene resin 2 and carbon black masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0130] (3) Cross-linking and plasticization:
[0131] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0132] Comparative Example 2 (the main difference from Example 1 is that the amount of esterified carbon black masterbatch added to material B is 25 parts) Preparation of esterified carbon black masterbatch:
[0133] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0134] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0135] Insulation material preparation:
[0136] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0137] Raw materials of material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 25 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0138] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0139] (1) Preparation of material A:
[0140] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0141] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0142] ③ After adding the esterified carbon black masterbatch, the mixture is extruded into granules and dried through a single screw extruder; the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0143] (2) Preparation of material B:
[0144] ① Polyethylene resin 1, polyethylene resin 2 and esterified carbon black masterbatch were dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst were added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0145] (3) Cross-linking and plasticization:
[0146] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0147] Comparative Example 3 (the main difference from Example 1 is that the amount of esterified carbon black masterbatch added to material B is 45 parts) Preparation of esterified carbon black masterbatch:
[0148] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0149] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0150] Insulation material preparation:
[0151] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0152] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 45 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0153] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0154] (1) Preparation of material A:
[0155] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0156] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0157] ③ After adding the esterified carbon black masterbatch, the mixture is extruded into granules and dried through a single screw extruder; the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0158] (2) Preparation of material B:
[0159] ① Polyethylene resin 1, polyethylene resin 2 and esterified carbon black masterbatch were dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst were added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0160] (3) Cross-linking and plasticization:
[0161] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0162] Comparative Example 4 (the main difference from Example 1 is that the amount of esterified carbon black masterbatch added in material A is 15 parts) Preparation of esterified carbon black masterbatch:
[0163] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0164] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0165] Insulation material preparation:
[0166] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 15 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0167] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0168] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0169] (1) Preparation of material A:
[0170] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0171] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0172] ③ After adding the esterified carbon black masterbatch, the mixture is extruded into granules and dried through a single screw extruder; the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0173] (2) Preparation of material B:
[0174] ① Polyethylene resin 1, polyethylene resin 2 and esterified carbon black masterbatch were dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst were added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0175] (3) Cross-linking and plasticization:
[0176] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0177] Comparative Example 5 (the main difference from Example 1 is that the carbon black surface is not hydroxymethylated when preparing the esterified carbon black masterbatch)
[0178] Preparation of modified carbon black masterbatch:
[0179] S1: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain modified carbon black masterbatch.
[0180] Insulation material preparation:
[0181] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of modified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0182] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of modified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0183] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0184] (1) Preparation of material A:
[0185] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0186] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0187] ③ After adding the modified carbon black masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0188] (2) Preparation of material B:
[0189] ① Polyethylene resin 1, polyethylene resin 2 and modified carbon black masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0190] (3) Cross-linking and plasticization:
[0191] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0192] Comparative Example 6 (the main difference from Example 1 is that the reaction base liquid is not ultrasonicated when preparing the modified carbon black masterbatch)
[0193] Preparation of modified carbon black masterbatch:
[0194] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0195] S2: Dissolve maleic anhydride in DMSO, add perchloric acid and mix well to obtain a reaction base liquid, wherein the molar volume ratio of maleic anhydride, perchloric acid and DMSO in the reaction base liquid is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain modified carbon black masterbatch.
[0196] Insulation material preparation:
[0197] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of modified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0198] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of modified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0199] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0200] (1) Preparation of material A:
[0201] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0202] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0203] ③ After adding the modified carbon black masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0204] (2) Preparation of material B:
[0205] ① Polyethylene resin 1, polyethylene resin 2 and modified carbon black masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0206] (3) Cross-linking and plasticization:
[0207] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0208] Comparative Example 7 (the main difference from Example 1 is that the reaction base liquid is ultrasonicated for 4 hours when preparing the modified carbon black masterbatch) Preparation of modified carbon black masterbatch:
[0209] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0210] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 4 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain modified carbon black masterbatch.
[0211] Insulation material preparation:
[0212] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of modified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0213] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of modified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0214] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0215] (1) Preparation of material A:
[0216] ① Mix the raw materials polyethylene resin 1, polyethylene resin 2 and polypropylene resin evenly and dry them to obtain a mixture;
[0217] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0218] ③ After adding the modified carbon black masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0219] (2) Preparation of material B:
[0220] ① Polyethylene resin 1, polyethylene resin 2 and modified carbon black masterbatch are dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst are added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0221] (3) Cross-linking and plasticization:
[0222] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0223] Comparative Example 8 (the main difference from Example 1 is that material A and material B are directly mixed together for mixing, extrusion and molding)
[0224] Preparation of esterified carbon black masterbatch:
[0225] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0226] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0227] Insulation material preparation:
[0228] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 10 parts of polypropylene resin, 7 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0229] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0230] Among them, the melting index of polyethylene resin 1 at 190°C and 2.16kg is 2.0±3g / 10min; the melting index of polyethylene resin 2 at 190°C and 2.16kg is 20±3g / 10min; and the melting index of polypropylene resin at 190°C and 2.16kg is 1.5±0.5g / 10min.
[0231] (1) Cross-linking and plasticization: Material A and material B are mixed in a mass ratio of 9:1, extruded and molded by a single screw extruder, and then rolled into a coil and placed in a steam chamber at 95°C for 4 hours to obtain an insulating material. The temperatures of each zone of the single screw extruder are shown in Table 4.
[0232] Comparative Example 9 (the main difference from Example 1 is that no polypropylene resin is added to material A)
[0233] Preparation of esterified carbon black masterbatch:
[0234] S1: Add 37 wt% formaldehyde solution to carbon black at a mass volume ratio of 7kg:7.2L, add NaOH to adjust the pH to 8.0, and react at 60°C for 3.5h to obtain hydroxymethylated carbon black.
[0235] S2: Dissolve maleic anhydride in DMSO, add perchloric acid, and ultrasonicate for 2 hours to obtain a reaction base liquid, in which the molar volume ratio of maleic anhydride, perchloric acid and DMSO is 0.8 mol:0.6 mol:1 L. Add hydroxymethylated carbon black to the reaction base liquid at a volume mass ratio of 1 L:1 kg, react at 75°C for 5 hours, dry and grind to obtain esterified carbon black masterbatch.
[0236] Insulation material preparation:
[0237] Raw materials of material A (parts by weight): 50 parts of polyethylene resin 1, 15 parts of polyethylene resin 2, 7 parts of esterified carbon black masterbatch, 1.8 parts of vinyl triethoxysilane, 0.20 parts of diisopropylbenzene peroxide, 0.18 parts of trimethoxymethane, and 0.08 parts of antioxidant 300.
[0238] Raw materials for material B (parts by weight): 25 parts of polyethylene resin 1, 25 parts of polyethylene resin 2, 4 parts of silicone powder, 0.8 parts of dibutyltin dilaurate, 3 parts of antioxidant 1010, 35 parts of esterified carbon black masterbatch, 0.8 parts of anti-copper agent 1024, 0.7 parts of phenyl o-hydroxybenzoate, and 0.8 parts of hindered amine light stabilizer.
[0239] The melt index of polyethylene resin 1 at 190° C. and 2.16 kg is 2.0±3 g / 10 min; the melt index of polyethylene resin 2 at 190° C. and 2.16 kg is 20±3 g / 10 min.
[0240] (1) Preparation of material A:
[0241] ① Evenly mix the raw materials polyethylene resin 1 and polyethylene resin 2, and dry them to obtain a mixture;
[0242] ② The silane coupling agent, dehydrating agent, initiator and antioxidant are mixed, stirred and dissolved, added into the mixture, and extruded and kneaded through a twin-screw extruder to obtain a mixed initial material; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 1.
[0243] ③ After adding carbon black modified masterbatch, granulation and drying are carried out through a single screw extruder; wherein, the temperature parameters of each zone of the single screw extruder are shown in Table 2.
[0244] (2) Preparation of material B:
[0245] ① Polyethylene resin 1, polyethylene resin 2 and carbon black modified masterbatch were dried, silicone powder, anti-ultraviolet absorber, light stabilizer, anti-copper agent, antioxidant and catalyst were added and mixed, and extruded, impregnated, granulated and dried through a twin-screw extruder; wherein, the temperature parameters of each zone of the twin-screw extruder are shown in Table 3.
[0246] (3) Cross-linking and plasticization:
[0247] ① Material A and material B were mixed in a mass ratio of 9:1, extruded and formed by a single screw extruder, and then wound into a coil and placed in a steam chamber for cross-linking at 95°C for 4 hours to obtain an insulating material. The temperature of each zone of the single screw extruder is shown in Table 4.
[0248] Performance Testing
[0249] The insulating materials prepared in Examples 1 to 3 and Comparative Examples 1 to 9 were subjected to comprehensive performance tests. The performance results before aging treatment are shown in Table 13, and the performance results after aging treatment are shown in Table 14. The aging treatment is specifically: heat aging in an air oven at 135°C for 168h. The impact embrittlement performance is tested at -76°C. Thermal extension test conditions: 200°C, 0.2MPa, 15min.
[0250] Table 13
[0251]
[0252]
[0253] Table 14
[0254]
[0255] Data analysis
[0256] (1) As shown in Table 13, the insulating materials prepared in Examples 1 to 3 have a high carbon black content of more than 3%, and can also maintain excellent mechanical strength and electrical strength, large margins in thermal elongation and thermal shrinkage performance indicators, and excellent weather resistance and electrical tracking resistance. As shown in Table 14, Examples 1 to 3 can still maintain good mechanical properties and electrical tracking resistance after aging treatment.
[0257] (2) Compared with Example 1, the carbon black material added in Comparative Example 1 is ordinary carbon black masterbatch, and its mechanical strength, electrical strength, and tracking resistance are deteriorated, and the performance is seriously reduced after aging, indicating that the esterified carbon black masterbatch prepared by the present invention is beneficial to improving the mechanical strength, electrical strength, weather resistance and tracking resistance of insulating materials.
[0258] (3) Compared with Example 1, the amount of esterified carbon black masterbatch added in the B material of Comparative Example 2 is 25 parts. The amount of esterified carbon black masterbatch added in the B material is too small, and its mechanical strength, electrical strength, and electrical tracking resistance are deteriorated, and the performance decreases after aging, indicating that the addition of too little esterified carbon black masterbatch in the B material has no significant effect on improving the mechanical strength, electrical strength, weather resistance and electrical tracking resistance of the insulating material.
[0259] (4) Compared with Example 1, the amount of esterified carbon black masterbatch added in the B material of Comparative Example 3 is 45 parts. The amount of esterified carbon black masterbatch added in the B material is too much, and its mechanical strength, electrical strength, and electrical tracking resistance are deteriorated, and the performance decreases after aging. This shows that the excessive amount of esterified carbon black masterbatch added in the B material is not conducive to improving the mechanical strength and electrical strength of the insulating material, and the improvement of weather resistance and electrical tracking performance is not significant. Combined with Comparative Example 2, it is further explained that the amount of esterified carbon black masterbatch added in the B material must be within an appropriate range, and its addition amount has an optimal range value for improving the mechanical strength, electrical strength, weather resistance and electrical tracking performance of the insulating material.
[0260] (5) Compared with Example 1, the amount of esterified carbon black masterbatch added in the material A of Comparative Example 4 is 15 parts. The amount of esterified carbon black masterbatch added in the material A is too much, and its mechanical strength, electrical strength, and electrical tracking resistance are deteriorated, and the performance decreases after aging, indicating that the amount of esterified carbon black masterbatch added in the material A should not be too much.
[0261] (6) Compared with Example 1, when preparing the esterified carbon black masterbatch in Comparative Example 5, the carbon black surface is not hydroxymethylated, and its mechanical strength, electrical strength, and tracking resistance are deteriorated, and the performance is seriously reduced after aging, indicating that the preparation of the modified carbon black masterbatch requires surface hydroxymethylation and then maleic anhydride grafting. The esterified carbon black masterbatch prepared by first surface hydroxymethylation and then maleic anhydride grafting is beneficial to improving the performance of insulating materials.
[0262] (7) Compared with Example 1, when preparing the modified carbon black masterbatch in Comparative Example 6, the reaction base liquid was not ultrasonicated, and its mechanical strength, electrical strength, and tracking resistance deteriorated, and the performance decreased after aging treatment. This shows that before the maleic anhydride grafting of the modified carbon black masterbatch, ultrasound is beneficial to the activation of maleic anhydride, which is beneficial to the esterified carbon black masterbatch prepared by grafting, thereby improving the performance of the insulating material.
[0263] (8) Compared with Example 1, when preparing the modified carbon black masterbatch in Comparative Example 7, the reaction base liquid was ultrasonicated for 4 hours. The ultrasonication time was too long, and its mechanical strength, electrical strength, and tracking resistance deteriorated, and the performance decreased after aging treatment, indicating that the reaction base liquid ultrasonication time was too long, which had an inhibitory effect on maleic anhydride.
[0264] (9) Compared with Example 1, in Comparative Example 8, material A and material B are directly mixed together for kneading, extrusion and molding. The mechanical strength, electrical strength and tracking resistance of the material are deteriorated, and the performance is seriously degraded after aging.
[0265] (10) Compared with Example 1, no polypropylene resin is added to the material of Comparative Example 9A, and 20 parts of polypropylene resin are added to the material of Comparative Example 10A. The polypropylene resin content is too high, and the strength and heat resistance of the insulating materials of Comparative Examples 9 and 10 are reduced, indicating that adding an appropriate amount of polypropylene resin can improve the strength and heat resistance of the prepared insulating material.
[0266] The polyethylene resin 1 used in the above examples and comparative examples is the same polyethylene resin. The polyethylene resin 2 used in the above examples and comparative examples is the same polyethylene resin.
[0267] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0268] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material, characterized in that: Included steps ①Material A By weight, 40-60 parts of polyethylene resin 1, 10-20 parts of polyethylene resin 2 and 5-15 parts of polypropylene resin are mixed evenly and dried to obtain a mixture; 1.5-2 parts of silane coupling agent, 0.12-0.21 parts of dehydrating agent, 0.13-0.23 parts of initiator and 0.04-0.11 parts of antioxidant are mixed evenly and dissolved, and added to the mixture for kneading to obtain a preliminary kneading material; 3-8 parts of esterified carbon black masterbatch are added for extrusion granulation and drying; the melt indexes of polyethylene resin 1 and polyethylene resin 2 at 190°C and 2.16kg are 2.0±3 g / 10min and 20±3 g / 10min respectively; Add formaldehyde solution to carbon black, adjust pH with NaOH, and react to obtain hydroxymethylated carbon black; dissolve maleic anhydride in DMSO, add perchloric acid and ultrasonicate for 2-3h, then add hydroxymethylated carbon black to react, dry and grind to obtain esterified carbon black masterbatch; ②Material B 20-30 parts of polyethylene resin 1, 20-30 parts of polyethylene resin 2 and 30-40 parts of esterified carbon black masterbatch are dried, 3-5 parts of silicone powder, 0.5-1 parts of anti-ultraviolet absorber, 0.5-1 parts of light stabilizer, 0.5-1 parts of anti-copper agent, 2-4 parts of antioxidant and 0.5-1 parts of catalyst are added and mixed, extruded, impregnated, granulated and dried; ③ Cross-linking plasticization The material A and the material B are mixed in a mass ratio of 90-95:5-10, molded, and cross-linked to obtain an insulating material.
2. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The polypropylene resin has a melt index of 1.5±0.5 g / 10 min at 190° C. and 2.16 kg.
3. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The silane coupling agent is one or more of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl tri(β-methoxyethoxy)silane.
4. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The initiator is dicumyl peroxide.
5. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The dehydrating agent is trimethoxymethane.
6. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate.
7. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 300, antioxidant 1076, antioxidant 1010, antioxidant AT 10, antioxidant DSTP and antioxidant DLTP.
8. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: In step ①, the mixing is carried out by a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are: Ⅰ 118-122°C, Ⅱ 138-142°C, Ⅲ 123-127°C, Ⅳ 178-182°C, Ⅴ 193-197°C, Ⅵ 198-202°C, Ⅶ 198-202°C, VIII 198-202°C, IX 198-202°C, and the head is 188-192°C.
9. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 1, characterized in that: The extrusion granulation is carried out by a single screw extruder, and the temperature of each zone of the single screw extruder is: Ⅰ 143~147℃, Ⅱ 163~167℃, and the head 173~177℃.
10. The method for preparing a weather-resistant and electric-track-resistant silane cross-linked polyethylene insulating material according to claim 8 or 9, characterized in that: In step ②, the extrusion is carried out by a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are: I 58-62°C, II 138-142°C, III 178-182°C, IV 148-152°C, V 188-192°C, VI 188-192°C, VII 188-192°C, VIII 188-192°C, IX 188-192°C, and the head 178-182°C.