A laminated composite photocatalyst with mesoporous membrane and its preparation method and application
By using a laminated composite structure of mesoporous membranes in the photocatalyst, the problems of single conductivity and adsorption of existing photocatalysts are solved, and efficient, stable and low-cost photolysis of water to produce hydrogen is achieved, and the hydrogen production is significantly increased. .
Patent Information
- Application Number
- CN202310097119.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When existing photocatalysts photolyze water to produce hydrogen, they have single conductivity and adsorption effects, are high in cost, and are difficult to achieve efficient, stable, and low-cost photocatalytic water splitting reactions.
A laminated composite photocatalyst with a mesoporous membrane is used, which is composed of a carrier matrix (layered Ti3C2 nanosheets), a surface coating (mesoporous membrane) and a binder (perfluorosulfonic acid resin), and is formed through a specific preparation method The laminated structure improves the conductivity and reactivity of the photocatalyst.
Efficient, stable and low-cost photocatalytic water splitting is achieved to produce hydrogen. The photocatalyst has excellent conductivity and hydrophilicity. The pore structure promotes cascade reactions, improves the photocatalytic efficiency, and the hydrogen production reaches more than 1000 μmol.
Smart Images

Figure CN116273102B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photocatalysts and preparation thereof, in particular to a laminated composite photocatalyst with a mesoporous membrane and a preparation method and application thereof. Background Art
[0002] Compared to traditional fossil fuels, hydrogen energy has attracted considerable attention due to its high efficiency and cleanliness. Scientists worldwide are racing to develop hydrogen-related technologies and products. Rapid, efficient, and affordable hydrogen production is crucial for the advent of a hydrogen economy. Traditional hydrogen production methods primarily involve cracking coal, oil, or natural gas, or through water electrolysis. Because hydrogen production consumes significant amounts of fossil fuels and contributes to regional environmental pollution and global warming, developing green and clean hydrogen production methods has become a key goal of hydrogen energy development.
[0003] Solar energy and water are two important renewable resources on Earth. Using solar energy to decompose water to produce hydrogen is the cleanest way to produce hydrogen and has always been the dream of mankind to develop hydrogen energy. Therefore, the research on new photocatalysts for photocatalytic water splitting to produce hydrogen is the future development direction. Bismuth vanadate (BiVO4) is considered to be one of the most promising photoanode materials for photocatalytic water splitting to produce hydrogen. The band gap of BiVO4 is 2.4 eV. Under the illumination of AM 1.5 G (100 mW / cm 2 ), the theoretical photocurrent density that can be achieved is 7.5 mA / cm 2 , corresponding to a solar-to-hydrogen (STH) efficiency of 9.2%. Although BiVO4's band gap is slightly larger than the ideal band gap of 2.0 eV for photoelectric water splitting, its conduction band edge is located very close to the H2 evolution potential. Therefore, compared with many other photoanode materials, BiVO4 has a lower onset potential and higher photocurrent density in the low-potential region. Researchers at Osaka University in Japan have combined two-dimensional black phosphorus (BP) and BiVO4 to prepare a novel two-dimensional BP / BiVO4 composite heterojunction catalyst. This composite catalyst exhibits a wide spectral response from ultraviolet to visible light and excellent electron-hole separation performance, achieving excellent photoelectric water-to-hydrogen efficiency without sacrificing agents or additional energy consumption. Separately, researchers at Tianjin University have controllably introduced oxygen vacancies onto the BiVO4 photoanode surface through photolithography, significantly enhancing the BiVO4's photoelectric activity. After optimizing the BiVO4 electrode thickness and loading it with additives, the BiVO4 electrode was connected in series with a silicon cathode to achieve a highly efficient, bias-free self-water splitting device with a solar energy conversion efficiency of up to 3.5%.
[0004] CN201710351559 discloses a method for constructing a photoelectrochemical sensor for enzyme-free detection of dopamine. This patent successfully establishes a photoelectrochemical sensing platform by preparing a BiOCl / BiVO4 / nitrogen graphene quantum dot (N-GQDs) nanocomposite as the photoelectroactive material. The BiOCl / BiVO4 / N-GQDs nanocomposite's high visible light absorption and rapid response properties serve as a signal amplification for the detection system. A photoelectrochemical sensor for rapid and sensitive dopamine detection was constructed for enzyme-free photoelectrochemical detection of dopamine in human serum. A corresponding relationship between dopamine concentration and photocurrent response was established, achieving simple, sensitive, and rapid dopamine detection. Therefore, the prepared sensor can be used to detect dopamine levels in human serum.
[0005] CN201811361797 discloses a method for preparing Fe3O4 quantum dot-modified BiOCl / BiVO4 that responds to visible light. A visible light-responsive Fe3O4 quantum dot-modified BiOCl / BiVO4 composite photocatalyst was obtained. The Fe3O4 quantum dot-modified BiOCl / BiVO4 pn heterojunction was prepared using a simple and rapid method. The BiOCl / BiVO4 pn heterojunction showed excellent photocatalytic activity in the degradation of multiple antibiotics under visible light. The sample also had strong magnetism and was easily recyclable and reused.
[0006] CN202010215888.6 discloses a method for preparing a carbon cloth-loaded BiOCl / BiVO4 recyclable flexible composite photocatalytic material and its application. The carbon cloth-loaded BiOCl / BiVO4 recyclable flexible composite photocatalytic material uses easily available carbon cloth as a substrate, exhibits excellent conductivity, flexibility, and bendability, and there is no need to worry about material damage even if it is folded for a long time or bent repeatedly. It can also be cut according to different usage environments. It has the advantages of high carrier diffusion rate, wide light response range, recyclability, good cycle performance, and low cost. It improves the shortcomings of BiOCl's low light absorption and large energy loss, and solves the problem of difficult separation and recycling of powdered photocatalysts, thereby realizing sustainable development and recycling of resources.
[0007] CN202110064257.3 discloses a composite material of modified diatomite loaded with BiVO4-BiOCl heterojunction, in which rich amino and imino groups are introduced onto the surface of the diatomite. A large number of amino and imino groups can serve as active adsorption sites, so that the modified diatomite can effectively adsorb pollutants such as tetracycline through hydrogen bonding and electrostatic effects, thereby realizing the functional modification of the diatomite. BiOCl nanoflowers and Zn-doped mesoporous BiVO4 form a pn heterojunction, which promotes the separation of photogenerated electrons and holes, and further reacts with water to generate active substances such as hydroxyl radicals and superoxide radicals. First, the modified diatomite effectively adsorbs tetracycline through hydrogen bonding and electrostatic effects, and then photocatalytically degrades it into non-toxic small molecules, thereby realizing efficient adsorption and photocatalytic degradation of tetracycline.
[0008] Although all of the above-mentioned photocatalysts are composite photocatalysts, they are ternary composite photocatalysts constructed with nitrogen-doped graphene quantum dots, Fe3O4 quantum dots, carbon cloth and modified diatomaceous earth and BiVO4-BiOCl heterostructures. Among them, nitrogen-doped graphene quantum dots, Fe3O4 quantum dots and carbon cloth can enhance conductivity, while modified diatomaceous earth can enhance adsorption. Their respective performances are relatively simple and the cost is high. Summary of the Invention
[0009] In order to solve the above technical problems, the present invention provides a laminated composite photocatalyst with a mesoporous membrane that has high activity, good stability, and low cost and is suitable for the photocatalytic decomposition of water to produce hydrogen, as well as a preparation method and application thereof.
[0010] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0011] The first object of the present invention is to provide a laminated composite photocatalyst with a mesoporous membrane, wherein the composite photocatalyst is composed of a carrier matrix, a surface coating and a binder, and its structure is a laminated structure; the weight percentage of the carrier matrix in the composite photocatalyst is 68.0 to 99.0%, the weight percentage of the surface coating in the composite photocatalyst is 0.5 to 30.0%, and the weight percentage of the binder in the composite photocatalyst is 0.5 to 2.0%.
[0012] Preferably, the weight percentage of the carrier matrix in the composite photocatalyst is 84.0-94.5%, the weight percentage of the surface coating in the composite photocatalyst is 5.0-15.0%, and the weight percentage of the binder in the composite photocatalyst is 0.5-1.0%.
[0013] Preferably, the carrier matrix is a layered Ti3C2 nanosheet, and the thickness of a single sheet in the layered structure of the layered Ti3C2 nanosheet is 1 to 200 nm.
[0014] Preferably, the surface coating is a mesoporous membrane, and the pore size of the mesoporous membrane is 2 to 40 nm.
[0015] Preferably, the binder is perfluorosulfonic acid resin.
[0016] The first object of the present invention is to provide a method for preparing a laminated composite photocatalyst having a mesoporous membrane, comprising the following steps:
[0017] (1) Add 40-100 mL of 40-60% hydrofluoric acid into a plastic beaker, weigh 5-10 g of Ti3AlC2 and mix it. In order to mix it evenly, stir the mixed solution for 20-60 min. Then transfer the mixed solution to a stainless steel reactor for further reaction. After centrifugation, use a vacuum drying oven at 80-160 °C to treat it. Finally, cool the material to obtain the carrier matrix layered Ti3C2 nanosheets.
[0018] (2) Weigh 9-40 mg of Bi(NO3)3•5H2O and dissolve it in 10-60 mL of 1-4 mol / L dilute nitric acid, then add 2-18 mg of ammonium vanadate, stir magnetically at room temperature for 10-60 min, adjust the pH value of the solution system to 3-6 with dilute hydrochloric acid, weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and add the binder and continue stirring for 10-60 min. After the stirring is completed, transfer the liquid to a reactor and react at 100-180 °C for 12-48 h; then cool the material at room temperature, wash it with distilled water and ethanol two to three times respectively; then place the obtained product in a vacuum drying oven, adjust the temperature to 60-120 °C and dry it under vacuum for 8-24 h; finally, transfer the obtained powder to a tube furnace and calcine it at 350-550 °C under argon protection for 6-12 h. h is to prepare a laminated composite photocatalyst with a mesoporous film.
[0019] The third object of the present invention is to provide a laminated composite photocatalyst having a mesoporous membrane for use in photocatalytic water decomposition to produce hydrogen.
[0020] The photocatalytic principle of the laminated composite photocatalyst with a mesoporous membrane of the present invention is: it has an open structure, a high specific surface area, excellent conductivity, and visible light response. After light irradiation, it produces a large number of high-energy electrons that can participate in chemical reactions. At the same time, the mesoporous membrane structure has a large number of intimate heterojunctions that effectively inhibit the recombination of photogenerated electrons and holes, thereby improving the photocatalytic efficiency.
[0021] Compared with the prior art, the present invention prepares a mesoporous laminated composite photocatalyst that has both strong conductivity and hydrophilicity, wherein the carrier matrix Ti3C2 and the binder perfluorosulfonic acid resin have extremely strong conductivity and good hydrophilicity. In addition, the photocatalyst active components are BiVO4 and BiOCl nanoparticles, which form a film on the surface of each layer of Ti3C2 to form a laminated structure. The rich pore structure contributes to the occurrence of cascade reactions, increases the active sites of photocatalytic reactions inside the pores, and thus improves the photocatalytic efficiency. In addition, the porous open structure is conducive to the transmission of reactants and can also improve the photocatalytic efficiency. In addition, the mesoporous film laminated structure composite photocatalyst is not a simple superposition of the original performance, but a new material with an open structure, hydrophilicity, high conductivity, and visible light response, which makes its photoelectric performance qualitatively changed, and it has new functional characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is an SEM photograph of the carrier matrix layered Ti3C2 nanosheets prepared according to one embodiment of the present invention.
[0023] Figure 2 XRD spectrum of layered Ti3C2 nanosheets prepared according to one embodiment of the present invention.
[0024] Figure 3 XRD spectrum of the composite photocatalyst prepared according to one embodiment of the present invention.
[0025] Figure 4 An SEM photograph of a composite photocatalyst prepared according to one embodiment of the present invention.
[0026] Figure 5 TEM image of a composite photocatalyst prepared according to one embodiment of the present invention.
[0027] Figure 6 A pore size distribution curve of a composite photocatalyst prepared according to one embodiment of the present invention. Implementation Method
[0028] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0029] Unless otherwise specified, the materials and reagents used in the following examples are all commercially available, and their specific sources are not described in detail in the following examples. Example 1
[0030] (1) Weigh 10 g of Ti3AlC2 material, add 100 mL of 50% hydrofluoric acid, mix them evenly, stir the mixed solution for 60 min, then transfer the mixed solution to a stainless steel reactor for further reaction. After centrifugation, use a vacuum drying oven at 120 °C to treat it. Finally, cool the material to obtain the carrier matrix layered Ti3C2 nanosheets.
[0031] (2) Weigh 9.7 mg of Bi(NO3)3•5H2O and dissolve it in 20 mL of 2 mol / L dilute nitric acid. Then add 2.3 mg of NH4VO3 and stir magnetically at room temperature for 60 min. Use dilute hydrochloric acid to adjust the pH value of the solution system to 5. Weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and add 1 μL of binder and continue stirring for 30 min. After stirring, transfer the liquid to a reactor and react at 160 °C for 24 h. Then cool the material at room temperature. After cooling, wash it with distilled water and ethanol two to three times respectively. Then place the obtained product in a vacuum drying oven, adjust the temperature to 120 °C and dry it under vacuum for 12 h. Finally, transfer the obtained powder to a tube furnace and calcine it at 400 °C for 8 h under argon protection to obtain the final product A. Example 2
[0032] (1) Weigh 10 g of Ti3AlC2 material, add 100 mL of 50% hydrofluoric acid, mix them evenly, stir the mixed solution for 60 min, then transfer the mixed solution to a stainless steel reactor for further reaction. After centrifugation, use a vacuum drying oven at 120 °C to treat it. Finally, cool the material to obtain the carrier matrix layered Ti3C2 nanosheets.
[0033] (2) Weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and disperse them in 10 mL of anhydrous ethanol solution. Perform ultrasonic dispersion for 30 min. Then weigh 19.4 mg of Bi(NO3)3•5H2O and dissolve it in 20 mL of 2 mol / L dilute nitric acid. Then add 4.6 mg of NH4VO3 and stir magnetically at room temperature for 60 min. Use dilute hydrochloric acid to adjust the pH value of the solution system to 5. Then weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and add 1.2 μL of binder and continue stirring for 30 min. After stirring, transfer the liquid to a reactor and react at 160 °C for 24 h. Then cool the material at room temperature. After cooling, wash it with distilled water and ethanol two to three times respectively. Then place the obtained product in a vacuum drying oven, adjust the temperature to 120 °C and dry it under vacuum for 12 h. Finally, the obtained powder was transferred to a tube furnace and calcined at 400 °C for 8 h under argon protection to obtain the final product B. Example 3
[0034] (1) Weigh 10 g of Ti3AlC2 material, add 100 mL of 50% hydrofluoric acid, mix them evenly, stir the mixed solution for 60 min, then transfer the mixed solution to a stainless steel reactor for further reaction. After centrifugation, use a vacuum drying oven at 120 °C to treat it. Finally, cool the material to obtain the carrier matrix layered Ti3C2 nanosheets.
[0035] (2) Weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and disperse them in 10 mL of anhydrous ethanol solution. Perform ultrasonic dispersion for 30 min. Then weigh 29.1 mg of Bi(NO3)3•5H2O and dissolve it in 20 mL of 2 mol / L dilute nitric acid. Then add 6.9 mg of NH4VO3 and stir magnetically at room temperature for 60 min. Use dilute hydrochloric acid to adjust the pH value of the solution system to 5. Then weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and add 1.4 μL of binder and continue stirring for 30 min. After stirring, transfer the liquid to a reactor and react at 160 °C for 24 h. Then cool the material at room temperature. After cooling, wash it with distilled water and ethanol two to three times respectively. Then place the obtained product in a vacuum drying oven, adjust the temperature to 120 °C and dry it under vacuum for 12 h. Finally, the obtained powder was transferred to a tube furnace and calcined at 400 °C for 8 h under argon protection to obtain the final product C. Example 4
[0036] (1) Weigh 10 g of Ti3AlC2 material, add 100 mL of 50% hydrofluoric acid, mix them evenly, stir the mixed solution for 60 min, then transfer the mixed solution to a stainless steel reactor for further reaction. After centrifugation, use a vacuum drying oven at 120 °C to treat it. Finally, cool the material to obtain the carrier matrix layered Ti3C2 nanosheets.
[0037] (2) Weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and disperse them in 10 mL of anhydrous ethanol solution. Perform ultrasonic dispersion for 30 min. Then weigh 38.8 mg of Bi(NO3)3•5H2O and dissolve it in 20 mL of 2 mol / L dilute nitric acid. Then add 9.2 mg of NH4VO3 and stir magnetically at room temperature for 60 min. Use dilute hydrochloric acid to adjust the pH value of the solution system to 5. Then weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1) and add 1.6 μL of binder and continue stirring for 30 min. After stirring, transfer the liquid to a reactor and react at 160 °C for 24 h. Then cool the material at room temperature. After cooling, wash it with distilled water and ethanol two to three times respectively. Then place the obtained product in a vacuum drying oven, adjust the temperature to 120 °C and dry it under vacuum for 12 h. Finally, the obtained powder was transferred to a tube furnace and calcined at 400 °C for 8 h under argon protection to obtain the final product D.
[0038] The carrier matrix layered Ti3C2 nanosheets prepared in Example 4 and the final product D were used as examples for testing.
[0039] Figure 1 The SEM photo of the carrier matrix layered Ti3C2 nanosheet prepared in Example 4. Figure 1 It can be seen that the Ti3C2 material shows a layered structure under a high-power scanning electron microscope, and the thickness of its layered two-dimensional nanosheets is less than 50 nm.
[0040] Figure 2 XRD spectrum of the layered Ti3C2 nanosheets prepared in Example 4. Figure 2 It can be seen that the Ti3C2 material shows a Ti3C2 peak in the X-ray diffraction spectrum.
[0041] Figure 3 is the XRD spectrum of the final product D. Figure 3 It can be seen that the composite photocatalyst shows BiVO4, BiOCl and Ti3C2 peaks in the X-ray diffraction spectrum.
[0042] Figure 4This is the SEM photo of the final product D. Figure 4 It can be seen that the composite photocatalyst appears as a stacked structure under a high-power scanning electron microscope, in which the surface of the carrier matrix Ti3C2 is evenly covered by the mesoporous film.
[0043] Figure 5 This is the TEM picture of the final product D. Figure 5 It can be seen that the composite photocatalyst shows under high magnification transmission electron microscopy that the mesoporous film on the Ti3C2 surface is composed of BiVO4 and BiOCl particles less than 10 nm.
[0044] Figure 6 is the pore size distribution curve of the final product D. Figure 6 It can be seen from the figure that the pore size distribution range of the composite photocatalyst is 2.5 to 20 nm, which is a mesoporous structure.
[0045] The mesoporous film laminated composite photocatalyst prepared in Examples 1 to 4 was used to photocatalytically decompose water to produce hydrogen, and the reaction conditions were as follows:
[0046] The mesoporous film laminated composite photocatalysts prepared in Examples 1 to 4 were placed in quartz bottles, 300 mL of distilled water was added, and 4 g of sodium sulfide and 2 g of sodium sulfite were dissolved therein as photocatalytic sacrificial agents. The light source used in the experiment was a 500 W xenon lamp simulating sunlight with a light intensity of 100 mW∙cm -2 Before the reaction, nitrogen was purged for 30 minutes. The photocatalytic reaction was then continued for 48 hours. The generated gas was collected, its volume measured, and its composition analyzed by gas chromatography. The hydrogen production of the mesoporous membrane laminate composite photocatalysts prepared in Examples 1-4 is shown in Table 1.
[0047] Table 1
[0048] Example sample Continuous reaction time (h) Hydrogen production (μmol) Example 1 Mesoporous film laminated composite photocatalyst A 48 1091 Example 2 Mesoporous film laminated composite photocatalyst B 48 1406 Example 3 Mesoporous film laminated composite photocatalyst C 48 1756 Example 4 Mesoporous film laminated composite photocatalyst D 48 1890
[0049] As shown in Table 1, the mesoporous film laminated composite photocatalyst of the present invention has high photocatalytic efficiency when used for photocatalytic decomposition of water to produce hydrogen. After catalysis by the photocatalyst of the present invention, the hydrogen production amount reaches more than 1000 μmol in 48 hours, which is significantly better than the photocatalyst of the prior art.
[0050] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. Any technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A laminated composite photocatalyst having a mesoporous film, characterized in that: The composite photocatalyst is composed of a carrier matrix, a surface coating and a binder, and has a laminated structure; the carrier matrix accounts for 68.0-99.0% of the weight of the composite photocatalyst, the surface coating accounts for 0.5-30.0% of the weight of the composite photocatalyst, and the binder accounts for 0.5-2.0% of the weight of the composite photocatalyst; the carrier matrix is a layered Ti3C2 nanosheet, and the thickness of a single sheet in the layered structure of the layered Ti3C2 nanosheet is 1-200 nm; the surface coating is a mesoporous membrane, and the pore size of the mesoporous membrane is 2-40 nm; the binder is a perfluorosulfonic acid resin; the preparation method of the laminated composite photocatalyst with a mesoporous membrane comprises the following steps: (1) Add 40-100 mL of 40-60% hydrofluoric acid into a plastic beaker, weigh 5-10 g of Ti3AlC2 and mix with it. In order to make it uniformly mixed, stir the mixed solution for 20-60 min, then transfer the mixed solution to a stainless steel reactor for further reaction, centrifuge and then use a vacuum drying oven at 80-160 ° C to treat, and finally cool the material to obtain a carrier matrix layered Ti3C2 nanosheet; (2) Weigh 9-40 mg of Bi(NO3)3•5H2O and dissolve it in 10-60 mL of 1-4 mol / L dilute nitric acid, then add 2-18 mg of ammonium vanadate, stir magnetically at room temperature for 10-60 min, adjust the pH value of the solution system to 3-6 with dilute hydrochloric acid, weigh 100 mg of the carrier matrix layered Ti3C2 nanosheets obtained in step (1), add the binder and continue stirring for 10-60 min. After stirring, transfer the liquid to a reactor and react at 100-180°C for 12-48 h. Then cool the material at room temperature. After cooling, wash it with distilled water and ethanol two to three times respectively. Then place the obtained product in a vacuum drying oven, adjust the temperature to 60-120°C and dry it under vacuum for 8-24 h. Finally, transfer the obtained powder to a tube furnace and calcine it at 350-550°C for 6-12 hours under argon protection. h that is, a laminated composite photocatalyst with a mesoporous film is obtained.
2. The laminated composite photocatalyst with a mesoporous film according to claim 1, characterized in that: The weight percentage of the carrier matrix in the composite photocatalyst is 84.0-94.5%, the weight percentage of the surface coating in the composite photocatalyst is 5.0-15.0%, and the weight percentage of the binder in the composite photocatalyst is 0.5-1.0%.
3. Use of the laminated composite photocatalyst with a mesoporous membrane as claimed in claim 1 in photocatalytic decomposition of water to produce hydrogen.
Citation Information
Patent Citations
A method for constructing an enzyme-free photoelectrochemical sensor for dopamine detection
CN107064264B
Preparation method of visible light-responsive Fe3O4 quantum dot-modified BiOCl / BiVO4
CN109331848A
Carbon cloth loaded BiOCl / BiVO4 recyclable flexible composite photocatalytic material, and preparation method and application thereof
CN111330602A
Modified diatomite loaded BiVO4-BiOCl heterojunction composite material and application thereof
CN112871187A
Two-dimensional nanosheet composite photocatalyst with bimetallic nanoparticles as heterojunction and preparation method thereof
CN106622322A