Photocatalyst of CuS supported on graphite-like carbon nitride and preparation method thereof
By loading CuS promoter on graphite-like carbon nitride, the problems of narrow spectral response range of g-C3N4 photocatalyst and high photogenerated carrier recombination rate are solved, and the photocatalytic activity is significantly improved and the CO2 reduction efficiency is improved. , suitable for a variety of environmental pollution fields.
Patent Information
- Application Number
- CN202310130818.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-17
AI Technical Summary
The narrow spectral response range and high photogenerated carrier recombination rate of g-C3N4 photocatalysts limit their photocatalytic activity and are difficult to effectively apply to CO2 reduction.
By loading CuS cocatalyst on graphite-like carbon nitride, CuS/g-C3N4 composite photocatalyst is prepared in one step by hydrothermal method, which expands the spectral response range and specific surface area, inhibits photogenerated carrier recombination, and improves CO2 reduction efficiency.
The photocatalytic activity is significantly improved, the spectral response range is expanded to 600nm, the apparent quantum yield is increased by about 2 times, the process is simple and the energy consumption is low, and it is suitable for CO2 reduction and degradation of organic pollutants in water.
Smart Images

Figure CN116273115B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photocatalysts, and in particular to a photocatalyst of CuS loaded on graphite-like carbon nitride and a preparation method thereof. Background Art
[0002] While traditional energy provides strong impetus for global common development, it also brings about environmental pollution and energy crisis with huge risks. Photocatalytic reduction of CO2 uses abundant solar energy as the only energy input to directly convert CO2 and H2O into hydrocarbon solar fuels. It is a green redox technology that has been widely studied and applied in the field of environmental pollution.
[0003] The band gap between the highest occupied molecular orbital (HOMO, +1.4V) and the lowest unoccupied molecular orbital (LUMO, -1.3V) of g-C3N4 (Chinese name: graphite-like carbon nitride) is 2.7eV, which allows it to respond to and absorb blue-violet light energy with a wavelength less than 475nm in solar radiation, and has great application potential in the photocatalytic reduction of CO2. However, g-C3N4 monomers usually have a high recombination rate of photogenerated carriers and a narrow spectral response range, which seriously hinders its photocatalytic activity and is not conducive to its practical application.
[0004] Therefore, how to improve the spectral response range of g-C3N4 photocatalyst and suppress the recombination rate of its photogenerated carriers to improve its photocatalytic activity is a current research hotspot. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a CuS-loaded graphite-like carbon nitride photocatalyst and a preparation method thereof. CuS, as a common co-catalyst, has a narrow energy band and can effectively capture photoexcited electrons on g-C3N4, inhibit the attachment of photogenerated carriers, and at the same time increase the specific surface area of the catalyst to broaden the spectral response, greatly enhancing the CO2 reduction efficiency.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing a photocatalyst of CuS supported on graphite-like carbon nitride, the specific steps are as follows:
[0008] S1, calcining melamine to obtain g-C3N4;
[0009] S2, dissolving the g-C3N4 obtained in step S1 in deionized water, and then adding (CH3COO)2Cu·H2O to obtain a mixed solution A;
[0010] S3, dissolving H2NCSNH2 in deionized water, and then adding it to the mixed solution A obtained in step S2 to obtain a mixed solution B;
[0011] S4. Subjecting the mixed solution B obtained in step S3 to a hydrothermal reaction to obtain a photocatalyst in which CuS is loaded on g-C3N4.
[0012] Furthermore, in step S1, the melamine powder is calcined for the first time to obtain a block product, and then the block product is ground into powder and calcined for the second time to obtain g-C3N4.
[0013] In the above, the first calcination temperature is 530-545° C., and the calcination time is 1-2 h;
[0014] The second calcination temperature is 550-560°C, and the calcination time is 0.5-1h.
[0015] Furthermore, in step S2, the g-C3N4 obtained in step S1 is ultrasonically dispersed in deionized water, and then (CH3COO)2Cu·H2O is added and stirred to obtain a mixed solution A.
[0016] Furthermore, in the above, the ultrasonic time is 0.5h.
[0017] Furthermore, in the above, the stirring time is 0.5h.
[0018] Furthermore, in step S2, the concentration of the g-C3N4 is 0.0071-0.0218 g / ml.
[0019] Furthermore, in step S2, the concentration of (CH3COO)2Cu·H2O is 0.0005-0.0055 g / ml.
[0020] Furthermore, in step S3, H2NCSNH2 is dissolved in deionized water, and then slowly dripped into the mixed solution A obtained in step S2, and a mixed solution B is obtained after stirring.
[0021] Furthermore, in the above, the stirring time is 5 hours.
[0022] Furthermore, in step S3, the concentration of H2NCSNH2 is 0.0001-0.0018 g / ml.
[0023] Furthermore, in step S4, the mixed solution B obtained in step S3 is subjected to a hydrothermal reaction, and the reaction product is centrifuged, washed, and dried to obtain a photocatalyst in which CuS is loaded on g-C3N4.
[0024] Furthermore, the centrifugation and washing are performed 4 times, and the drying temperature is 85-90°C.
[0025] Furthermore, in step S4, the hydrothermal reaction temperature is 185-190° C., and the hydrothermal reaction time is 8-11 h.
[0026] In addition, the present invention also provides a CuS-supported photocatalyst on graphite-like carbon nitride, which is prepared by the above method.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] 1. The present invention uses a hydrothermal method to prepare and regulate the synthesis of a CuS co-catalyst-loaded g-C3N4 composite photocatalyst in one step. The CuS co-catalyst-loaded g-C3N4 composite photocatalyst prepared by the present invention creates more interfaces for the effective transfer of photogenerated electrons and holes, limits the recombination of photogenerated carriers of g-C3N4, and the apparent quantum yield of the composite catalyst can be increased by about 2 times compared with pure g-C3N4;
[0029] 2. The CuS co-catalyst-loaded g-C3N4 composite photocatalyst prepared by the present invention uses CuS as a co-catalyst to further expand the specific surface area and light absorption range of g-C3N4. Its specific surface area is about 1.7 times that of pure g-C3N4, and the light absorption range can also be expanded from the original ~450nm to ~600nm;
[0030] 3. The CuS co-catalyst-loaded g-C3N4 composite photocatalyst prepared by the present invention has a simple process, a short synthesis cycle, low energy consumption, and readily available raw materials;
[0031] 4. The CuS co-catalyst loaded g-C3N4 composite photocatalyst prepared by the present invention is suitable for the reduction of carbon dioxide, the degradation of organic pollutants in water bodies, the decomposition of harmful microorganisms and bacteria, etc. It has a wide range of applications, is green and environmentally friendly, and is in line with the national strategic goal of energy conservation and emission reduction, and has important economic and social significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a SEM image of the CuS co-catalyst loaded g-C3N4 composite photocatalyst prepared in Example 1 of the present application;
[0033] Figure 2 This is a HRTEM image of the CuS co-catalyst loaded g-C3N4 composite photocatalyst prepared in Example 1 of the present application;
[0034] Figure 3 The photocatalytic reduction CO2 efficiency diagram of CuS co-catalyst loaded g-C3N4 composite photocatalyst and pure g-C3N4 obtained in Examples 1-3 of the present application;
[0035] Figure 4 This is a cyclic stability diagram of the CuS co-catalyst loaded g-C3N4 composite photocatalyst prepared in Example 2 of the present application. DETAILED DESCRIPTION
[0036] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0038] Secondly, the present application is described in detail with reference to the schematic diagram. When describing the embodiments of the present application in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present application. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.
[0039] Secondly, the "one embodiment" or "embodiment" referred to herein refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present application. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.
[0040] A method for preparing a photocatalyst of CuS supported on graphite-like carbon nitride, the specific steps are as follows:
[0041] S1, calcining melamine to obtain g-C3N4;
[0042] S2, dissolving the g-C3N4 obtained in step S1 in deionized water, and then adding (CH3COO)2Cu·H2O to obtain a mixed solution A;
[0043] S3, dissolving H2NCSNH2 in deionized water, and then adding it to the mixed solution A obtained in step S2 to obtain a mixed solution B;
[0044] S4. Subjecting the mixed solution B obtained in step S3 to a hydrothermal reaction to obtain a photocatalyst in which CuS is loaded on g-C3N4.
[0045] Furthermore, in step S1, the melamine powder is calcined for the first time to obtain a block product, and then the block product is ground into powder and calcined for the second time to obtain g-C3N4.
[0046] In the above, the first calcination temperature is 530-545° C., and the calcination time is 1-2 h;
[0047] The second calcination temperature is 550-560°C, and the calcination time is 0.5-1h.
[0048] Furthermore, in step S2, the g-C3N4 obtained in step S1 is ultrasonically dispersed in deionized water, and then (CH3COO)2Cu·H2O is added and stirred to obtain a mixed solution A.
[0049] Furthermore, in the above, the ultrasonic time is 0.5h.
[0050] Furthermore, in the above, the stirring time is 0.5h.
[0051] Furthermore, in step S2, the added amount of g-C3N4 is 0.6-1.2 g.
[0052] Furthermore, in step S2, the amount of deionized water added is 55-85 mL.
[0053] Furthermore, in step S2, the added amount of (CH3COO)2Cu·H2O is 0.04-0.3g.
[0054] Furthermore, in step S3, H2NCSNH2 is dissolved in deionized water, and then slowly dripped into the mixed solution A obtained in step S2, and a mixed solution B is obtained after stirring.
[0055] Furthermore, in the above, the stirring time is 5 hours.
[0056] Furthermore, in step S3, the added amount of H2NCSNH2 is 0.01-0.1g.
[0057] Furthermore, in step S3, the amount of deionized water added is 55-85 mL.
[0058] Furthermore, in step S4, the mixed solution B obtained in step S3 is subjected to a hydrothermal reaction, and the reaction product is centrifuged, washed, and dried to obtain a photocatalyst in which CuS is loaded on g-C3N4.
[0059] Furthermore, the centrifugation and washing are performed 4 times, and the drying temperature is 85-90°C.
[0060] Furthermore, in step S4, the hydrothermal reaction temperature is 185-190° C., and the hydrothermal reaction time is 8-11 h.
[0061] In addition, the present invention also provides a CuS-supported photocatalyst on graphite-like carbon nitride, which is prepared by the above method.
[0062] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0063] Example 1
[0064] like Figures 1 to 4 As shown, this embodiment provides a CuS-supported photocatalyst in a graphite-like carbon nitride phase, which is prepared by the following steps:
[0065] S1. Take melamine powder and add it into a ceramic crucible with a lid, and put it in a muffle furnace and calcine it at 530°C for 1 hour to obtain a block product. Then, after grinding the block product into powder, put it into a muffle furnace again and calcine it at 550°C for 0.5h. The product after calcination is g-C3N4.
[0066] S2. 0.6 g of g-C3N4 nanosheets obtained in step S1 were dispersed in 55 mL of deionized water by ultrasonication for 0.5 h, and then 0.04 g (CH3COO)2Cu·H2O was dissolved in the solution and stirred for 0.5 h to obtain a mixed solution A.
[0067] S3. Dissolve 0.01 g of H2NCSNH2 in 55 mL of deionized water, slowly drip it into the mixed solution A obtained in step S2, and stir vigorously for 5 h to obtain a mixed solution B.
[0068] S4. Pour the mixed solution B obtained in step S3 into multiple 100 mL polytetrafluoroethylene-lined autoclaves and hydroheat at 185°C for 8 h. After naturally cooling to room temperature, rinse with deionized water and anhydrous ethanol for 4 times respectively. Collect the resulting precipitate by centrifugation, place it in an oven at 85°C and dry it overnight to obtain the finished CuS / g-C3N4 photocatalyst.
[0069] Performance test: Take 50 mg of the prepared CuS / g-C3N4 photocatalyst, add 10 mL of triethanolamine (TEOA, 10 vol%) as an electron sacrificial agent and dissolve in 100 mL of deionized water, ultrasonically treat for 30 minutes, and then move to the reactor, and use the Labsolar-6A all-glass automatic online trace gas analysis system to test the photocatalytic CO2 reduction performance.
[0070] Example 2
[0071] This embodiment provides a CuS-supported graphite-like carbon nitride photocatalyst, which is prepared by the following steps:
[0072] S1. Take melamine powder and add it into a ceramic crucible with a lid, and place it in a muffle furnace and calcine it at 538°C for 1.5 hours to obtain a block product. Then, the block product is ground into powder and placed in a muffle furnace again and calcined at 555°C for 0.7 hours. The product after calcination is g-C3N4.
[0073] S2. 0.9 g of g-C3N4 nanosheets obtained in step S1 were dispersed in 70 mL of deionized water by ultrasonication for 0.5 h, and then 0.12 g of (CH3COO)2Cu·H2O was dissolved in the solution and stirred for 0.5 h to obtain a mixed solution A.
[0074] S3. Dissolve 0.05 g of H2NCSNH2 in 70 mL of deionized water, slowly drip it into the mixed solution A obtained in step S2, and stir vigorously for 5 h to obtain a mixed solution B.
[0075] S4. Pour the mixed solution B obtained in step S3 into multiple 100 mL polytetrafluoroethylene-lined autoclaves and hydroheat at 187°C for 9.5 h. After naturally cooling to room temperature, rinse with deionized water and anhydrous ethanol for 4 times respectively. Collect the resulting precipitate by centrifugation, place it in an oven at 87°C and dry it overnight to obtain the finished CuS / g-C3N4 photocatalyst.
[0076] Performance test: Take 50 mg of the prepared CuS / g-C3N4 photocatalyst, add 10 mL of triethanolamine (TEOA, 10 vol%) as an electron sacrificial agent and dissolve in 100 mL of deionized water, ultrasonically treat for 30 minutes, and then move to the reactor, and use the Labsolar-6A all-glass automatic online trace gas analysis system to test the photocatalytic CO2 reduction performance.
[0077] Example 3
[0078] This embodiment provides a CuS-supported graphite-like carbon nitride photocatalyst, which is prepared by the following steps:
[0079] S1. Take melamine powder and add it into a ceramic crucible with a lid, and place it in a muffle furnace and calcine it at 545°C for 2 hours to obtain a block product. Then, after grinding the block product into powder, put it into a muffle furnace again and calcine it at 560°C for 1 hour. The product after calcination is g-C3N4.
[0080] S2. Disperse 1.2 g of g-C3N4 nanosheets obtained in step S1 in 85 mL of deionized water by ultrasonication for 0.5 h, then dissolve 0.3 g of (CH3COO)2Cu·H2O in the solution and stir for 0.5 h to obtain a mixed solution A.
[0081] S3. Dissolve 0.1 g of H2NCSNH2 in 85 mL of deionized water, slowly drip it into the mixed solution A obtained in step S2, and stir vigorously for 5 h to obtain a mixed solution B.
[0082] S4. Pour the mixed solution B obtained in step S3 into multiple 100 mL polytetrafluoroethylene-lined autoclaves and hydroheat at 190°C for 11 h. After naturally cooling to room temperature, rinse with deionized water and anhydrous ethanol for 4 times respectively. Collect the resulting precipitate by centrifugation, place it in an oven at 90°C and dry it overnight to obtain the finished CuS / g-C3N4 photocatalyst.
[0083] Performance test: Take 50 mg of the prepared CuS / g-C3N4 photocatalyst, add 10 mL of triethanolamine (TEOA, 10 vol%) as an electron sacrificial agent and dissolve in 100 mL of deionized water, ultrasonically treat for 30 minutes, and then move to the reactor, and use the Labsolar-6A all-glass automatic online trace gas analysis system to test the photocatalytic CO2 reduction performance.
[0084] Conclusion Analysis
[0085] Reference Figure 1 , CuS spherical particles clearly appeared on the g-C3N4 nanosheets, indicating that CuS and g-C3N4 were successfully composited.
[0086] pass Figure 2 The HR-TEM further analyzed the microstructure of the CuS / g-C3N4 photocatalyst, and the lattice fringes with a lattice spacing of 0.328 nm in g-C3N4 were clearly observed, which belonged to the (100) crystal plane of CuS, which also proved that CuS was successfully loaded on the g-C3N4 surface.
[0087] Reference Figure 3 The figure shows that the main product of CO2 reduction in CuS / g-C3N4 composite photocatalyst is CO. With the different doping ratios, the generated CO yield is also changing, which effectively illustrates that CuS loaded g-C3N4 can effectively improve the photocatalytic performance. Example 2 has the best effect, and the CO yield reaches 14.95μmol.g -1 .cat -1 .
[0088] Reference Figure 4 , which shows that after three cycles, the CO yield only slightly decreased, indicating that the CuS / g-C3N4 composite material has good cycle stability.
[0089] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. Application of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide, It is characterized in that The preparation method of the photocatalyst is as follows: S1, calcining melamine powder for the first time to obtain a block product, then grinding the block product into powder and calcining it for the second time to obtain gC 3 N 4 ; The first calcination temperature is 530-545℃, and the calcination time is 1-2h. The second calcination temperature is 550-560°C and the calcination time is 0.5-1h; S2, gC obtained in step S1 3 N 4 Dissolve in deionized water and then add (CH 3 COO 2 Cu·H 2 O, to obtain a mixed solution A; S3, H 2 NCSNH 2 Dissolve in deionized water, and then add to the mixed solution A obtained in step S2 to obtain a mixed solution B; S4, subjecting the mixed solution B obtained in step S3 to a hydrothermal reaction, and subjecting the reaction product to centrifugation, washing, and drying to obtain CuS loaded on gC 3 N 4 photocatalyst; The hydrothermal reaction temperature is 185-190° C., and the hydrothermal reaction time is 8-11 hours.
2. Use of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step S2, gC obtained in step S1 is 3 N 4 Ultrasonic dispersion in deionized water, then adding (CH 3 COO 2 Cu·H 2 O, and obtain a mixed solution A after stirring; The gC 3 N 4 The concentration is 0.0071-0.0218 g / mL, The (CH 3 COO 2 Cu·H 2 The concentration of O is 0.0005-0.0055 g / mL.
3. Use of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide according to claim 2, It is characterized in that The ultrasonic time is 0.5h, The stirring time is 0.5h.
4. Use of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step S3, H 2 NCSNH 2 Dissolve in deionized water, and then slowly drip into the mixed solution A obtained in step S2, and stir to obtain a mixed solution B; The H 2 NCSNH 2 The concentration is 0.0001-0.0018 g / mL.
5. Use of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide according to claim 4, It is characterized in that The stirring time is 5h.
6. Use of a CuS-supported graphite-like carbon nitride photocatalyst for photocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that The centrifugation and washing were performed 4 times, and the drying temperature was 85-90°C.