A willow-leaf-shaped K-SUZ-4 molecular sieve and its preparation method
By controlling the hydrolysis and crystallization conditions during the synthesis of SUZ-4 molecular sieve, willow-like K-SUZ-4 molecular sieve was prepared, which solved the problems of low catalytic performance and single morphology, and achieved higher catalytic performance and better Broad applications.
Patent Information
- Application Number
- CN202310117843.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-15
AI Technical Summary
The existing SUZ-4 molecular sieve has low catalytic performance in catalytic reactions, especially the dimethyl ether conversion rate is relatively low, and it is generally single needle-shaped morphology, making it difficult to regulate the crystal growth direction and pore exposure.
A preparation method of willow-like K-SUZ-4 molecular sieve is adopted to realize SUZ- by controlling the hydrolysis of hydrochloric acid, ethyl orthosilicate, alkaline dissolution and silicon-aluminum mixed gel during the synthesis process. The controllable growth of 4 molecular sieve changes its aspect ratio and increases the eight-membered ring ratio to form a willow-like structure with a thickness less than 100nm, a large b-axis width and a high exposure ratio of eight-membered ring pores.
The thinner thickness of SUZ-4 molecular sieve and higher exposure to eight-membered ring pores were achieved, which improved catalytic performance and expanded its application potential in catalytic reactions.
Smart Images

Figure CN116282068B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve synthesis, and particularly relates to a willow-leaf-shaped K-SUZ-4 molecular sieve and a preparation method thereof. Background Art
[0002] SUZ-4 is a microporous zeolite that was first synthesized in 1992. Its topological structure is composed of four, five, six, eight and ten-membered rings. Among them, the ten-membered ring channel with the largest pore size is parallel to the c-axis and intersects with the two rows of eight-membered ring channels along the a-axis at 74°, forming its unique three-dimensional pores. Due to its unique pore structure, acidic characteristics and high hydrothermal stability, its application range in the fields of selective adsorption, separation and industrial catalysis has gradually expanded. In recent years, researchers have successively used SUZ-4 molecular sieves in reactions such as the conversion of n-hexane, the elimination of nitrogen oxides, the conversion of methanol to dimethyl ether and other hydrocarbons, the conversion of synthesis gas to olefins, the carbonylation of methanol and dimethyl ether, and the hydrogenation conversion of carbon dioxide.
[0003] Different pore structures of zeolite molecular sieves can show efficient catalytic shape selectivity in specific catalytic reactions. If the crystal growth mode is adjusted during the synthesis of molecular sieves to expose more specific pores, it will help to further improve the catalytic performance. In addition, the diffusion efficiency of reactants in the pores of molecular sieves is another factor affecting the catalytic performance of molecular sieves. Controlling the synthesis conditions to reduce the catalyst particle size or inhibiting the growth trend of crystals along a certain direction and reducing their thickness are conducive to increasing the diffusion efficiency and thus improving the catalytic performance. Taking the carbonylation reaction of dimethyl ether as an example, the shape selectivity of the eight-membered ring pores enables SUZ-4 molecular sieves to show good selectivity for methyl acetate products, and the lower side reactions in the ten-membered rings maintain a certain catalytic stability, but the overall dimethyl ether conversion rate is low, and there is still a distance from practical application, which requires further in-depth development. Therefore, based on the above understanding, improving the exposure of the eight-membered ring pores of SUZ-4, reducing the thickness of the molecular sieve and improving the diffusion efficiency are one of the effective means to improve catalytic performance and expand its application field.
[0004] At present, the growth regulation of SUZ-4 molecular sieves is mainly focused on the regulation of the overall morphology. For example, patent CN201910140480 reported that by changing the ratio of the mixed templates ethylenediamine (EDA) and cycloethylamine (CHA) in the synthesis system, a hedgehog-shaped SUZ-4 molecular sieve was synthesized; CN 109704364A reported that by adjusting the amount, ratio and addition time of the mixed solution of ethanol and acetic acid in the synthetic gel system, the molecular sieve was changed from a dispersed rod-like structure to a micron-shaped sphere similar to a dandelion or chrysanthemum. The above reports focus on the preliminary regulation of the overall morphology of SUZ-4 by changing the template or introducing an external surfactant, and have not yet specifically involved the growth of molecular sieve crystals along a certain direction and the exposure of pores. Summary of the invention
[0005] In view of the problem that the currently synthesized SUZ-4 molecular sieves are generally needle-shaped and have a single morphology, the present invention provides a willow-leaf-shaped K-SUZ-4 molecular sieve material and a preparation method thereof.
[0006] It is expected that without introducing other directing agents, the aspect ratio of the SUZ-4 molecular sieve can be changed, thereby increasing the proportion of the eight-membered ring and achieving controllable growth of the SUZ-4 crystal.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a willow-leaf-shaped K-SUZ-4 molecular sieve comprises the following steps:
[0009] Step 1, adding hydrochloric acid and tetraethyl orthosilicate (TEOS) to deionized water in sequence, stirring to fully hydrolyze, heating to evaporate part of the ethanol, and obtaining a uniform colloidal solution A;
[0010] Step 2, adding an alkali source (KOH) and an aluminum source to deionized water in sequence, transferring the mixture to a homogeneous reactor, heating the mixture to fully dissolve the mixture, taking the mixture out and cooling it to room temperature to obtain a uniform and stable solution B;
[0011] Step 3, adding the directing agent and solution A to solution B in sequence, and stirring vigorously to obtain a uniform silica-alumina mixed gel;
[0012] Step 4, after continued stirring and aging, the mixture is transferred into a hydrothermal reactor and subjected to dynamic crystallization in a homogeneous reactor, and the crystallization time and temperature are controlled to obtain a crystallized product containing a template SUZ-4 molecular sieve;
[0013] Step 5, washing, drying and calcining the obtained crystallized product to obtain a willow-leaf-shaped K-type SUZ-4 molecular sieve.
[0014] Furthermore, in the preparation of the colloidal solution A in step 1, TEOS needs to be hydrolyzed in a low concentration hydrochloric acid solution to prevent it from hydrolyzing too quickly and forming a gel-like solid. The molar ratio of the raw materials during the hydrolysis process is H2O:HCl:TEOS=(18-21):(0.015-0.06):(0.8-1.2)
[0015] Furthermore, in the preparation of the colloidal solution A in step 1, the solution formed after the hydrolysis is subjected to alcohol distillation treatment, the distillation temperature for heating and distilling off the ethanol is controlled at 40 to 60° C., stirring is continued during the distillation process, and the amount of distilled alcohol accounts for 21 wt.% to 32 wt.% of the total solution.
[0016] Furthermore, in step 2, the aluminum source is any one of aluminum powder, aluminum hydroxide, and aluminum isopropoxide, and the alkali source is KOH.
[0017] Furthermore, in the step 2, the molar ratio of raw materials in solution B is Al:KOH:H2O=1:(8-9.3):153; the dissolution temperature is 130-170°C, and the dissolution time is 2-5h.
[0018] Furthermore, in step 3, the directing agent is tetraethylammonium hydroxide (25% TEAOH).
[0019] Furthermore, the molar ratio of the raw materials in the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:(16-19):(18-24):(2-3):(618-671).
[0020] Furthermore, in step 4, the aging time is 2 to 5 hours, the speed of the homogeneous reactor is 15 to 20 rpm, the crystallization temperature is 160 to 180° C., and the crystallization time is 2 to 5 days.
[0021] Furthermore, in step 5, the drying temperature is 100-120° C. and the drying time is 5-8 hours; in step 5, the roasting temperature is 550-600° C., the roasting heating rate is 3° C. / min, and the roasting time is 6-10 hours.
[0022] A willow-leaf-shaped K-SUZ-4 molecular sieve prepared by the preparation method has a c-axis length of 3 μm, a b-axis width of 200 to 500 nm, and a thickness of less than 100 nm.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The present invention provides a synthesis process, in which only tetraethyl orthosilicate is used for hydrolysis and alcohol distillation to control the silicon source, and the raw material ratio and crystallization procedure are assisted to obtain a willow-leaf-shaped K-SUZ-4 molecular sieve with a c-axis length of about 3 μm, a b-axis width of about 200 to 500 nm, and a thickness of less than 100 nm. This process is simple, and without using expensive template agents, the synthesized K-SUZ-4 molecular sieve is thinner, has a large b-axis width, and has a high exposure ratio of the octagonal ring channels, which is expected to show better catalytic performance in specific reactions and obtain a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention is further described with reference to the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention.
[0026] Figure 1 is the XRD spectrum of the SUZ-4 molecular sieve catalyst;
[0027] Figure 2 is a SEM image of the molecular sieve catalyst obtained in Example 1 of the present invention;
[0028] Figure 3 This is a SEM image of the molecular sieve catalyst obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0029] Example 1
[0030] Step 1: First, fully hydrolyze TEOS, weigh 17g of TEOS in 25g of deionized water, add 4.8mL of 1M hydrochloric acid to the TEOS solution, and stir for 24h. Then put it in a water bath and heat to evaporate alcohol, the temperature of the alcohol is 50°C, the alcohol is evaporated for 3.5h, and the amount of alcohol evaporated is 14.2g, to obtain a uniform colloidal solution A.
[0031] Step 2, during the hydrolysis of TEOS, 1.92 g of KOH was weighed and dissolved in 10 g of deionized water, and then 0.835 g of aluminum hydroxide was added to the above solution. After stirring evenly, it was transferred to a stainless steel reactor and moved into a homogeneous reactor. It was dynamically dissolved at 170° C. for 3 h. After being taken out, it was cooled to room temperature in tap water. After opening the reactor, a uniform, stable and transparent solution B was obtained.
[0032] Step 3, then add 5.72g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring conditions. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel (the molar composition ratio of the gel is: Al2O3:KOH:SiO2:TEAOH:H2O=1:18.6:22:2.68:620).
[0033] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0034] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 , its SEM picture is shown in Figure 2 , it can be seen from the figure that the molecular sieve is willow-leaf shaped.
[0035] Example 2
[0036] Step 1: First, fully hydrolyze TEOS, weigh 17g of TEOS in 20g of deionized water, add 2.4mL of 1M hydrochloric acid to the TEOS solution, and stir for 24h. Then put it in a water bath and heat to evaporate alcohol, the temperature of the alcohol is 50°C, the alcohol is evaporated for 3.5h, and the amount of alcohol evaporated is 14.2g, to obtain a uniform colloidal solution A.
[0037] Step 2, during the hydrolysis of TEOS, 1.81 g of KOH was weighed and dissolved in 15 g of deionized water, and then 1.48 g of aluminum isopropoxide was added to the above solution. After stirring evenly, it was transferred to a stainless steel reactor and moved into a homogeneous reactor. It was dynamically dissolved at 150° C. for 5 h. After being taken out, it was cooled to room temperature in tap water. After opening the reactor, a uniform, stable and transparent solution B was obtained.
[0038] Step 3, then add 4.78g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring conditions. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel (the molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:16.4:22:2.24:626).
[0039] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0040] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 , its SEM picture is shown in Figure 3 , it can be seen from the figure that the molecular sieve is willow-leaf shaped.
[0041] Example 3
[0042] Step 1: First, fully hydrolyze TEOS. Weigh 15.5g of TEOS in 22g of deionized water, add 1.2mL of 1M hydrochloric acid to the TEOS solution, and stir for 24h. Stir for 24h. Then put it in a water bath and heat to evaporate alcohol. The temperature of the alcohol is 50°C, the alcohol is evaporated for 3.5h, and the amount of alcohol is 14.2g, to obtain a uniform colloidal solution A.
[0043] Step 2, during the hydrolysis of TEOS, 1.99 g KOH and 0.2 g aluminum powder were weighed and added to 13 g deionized water in sequence. A small amount of hydrogen was generated during the dissolution process and introduced into the room through a conduit until the aluminum powder was completely dissolved to obtain a uniform, stable and transparent solution B.
[0044] Step 3, then add 5.23g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel. The molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:18:20:2.45:618.
[0045] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0046] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 .
[0047] Example 4
[0048] Step 1: First, fully hydrolyze TEOS, weigh 16.2g of TEOS in 24g of deionized water, add 2.4mL of 1M hydrochloric acid to the TEOS solution, and stir for 12h. Then put it in a water bath and heat to evaporate alcohol, the temperature of the alcohol is 50°C, the alcohol is evaporated for 3.5h, and the amount of alcohol evaporated is 14.2g, to obtain a uniform colloidal solution A.
[0049] Step 2: During the hydrolysis of TEOS, 2.03 g of KOH was weighed and dissolved in 11 g of deionized water. Then, 0.835 g of aluminum hydroxide was added to the above solution. After stirring evenly, the mixture was transferred to a stainless steel reactor and then transferred to a homogeneous reactor. The mixture was dynamically dissolved at 160° C. for 5 h. After being taken out, the mixture was cooled to room temperature in tap water. After the reactor was opened, a uniform, stable and transparent solution B was obtained.
[0050] Step 3, then add 6.4g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel. The molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:18.4:21:3:642.
[0051] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0052] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 .
[0053] Example 5
[0054] Step 1: First, fully hydrolyze TEOS, weigh 18.5g of TEOS in 27g of deionized water, add 2.4mL of 1M hydrochloric acid to the TEOS solution, and stir for 5h. Then put it in a water bath and heat to evaporate alcohol, the temperature of the alcohol is 50°C, the alcohol is evaporated for 3.5h, and the amount of alcohol evaporated is 14.2g, to obtain a uniform colloidal solution A.
[0055] Step 2, during the hydrolysis of TEOS, 1.81 g of KOH was weighed and dissolved in 8 g of deionized water, and then 1.48 g of aluminum isopropoxide was added to the above solution. After stirring evenly, it was transferred to a stainless steel reactor and moved into a homogeneous reactor. It was dynamically dissolved at 170° C. for 3 h. After being taken out, it was cooled to room temperature in tap water. After opening the reactor, a uniform, stable and transparent solution B was obtained.
[0056] Step 3, then add 4.91g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel. The molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:16.4:24:2.3:637.
[0057] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0058] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 .
[0059] Example 6
[0060] Step 1: First, fully hydrolyze TEOS, weigh 17.8g of TEOS in 27g of deionized water, add 4.8mL of 1M hydrochloric acid to the TEOS solution, and stir for 24h. Then put it in a water bath and heat to evaporate alcohol, the temperature of the alcohol is 50°C, the alcohol is evaporated for 3h, and the amount of alcohol is 12g, to obtain a uniform colloidal solution A.
[0061] Step 2, during the hydrolysis of TEOS, 1.81 g KOH and 0.2 g aluminum powder were weighed and added to 12 g deionized water in sequence. A small amount of hydrogen was generated during the dissolution process and introduced into the room through a conduit until the aluminum powder was completely dissolved to obtain a uniform, stable and transparent solution B.
[0062] Step 3, then add 4.91g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel. The molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:16.4:23:2.68:620.
[0063] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0064] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 .
[0065] Example 7
[0066] Step 1: First, fully hydrolyze the silicon source TEOS, weigh 17g of TEOS in 21g of deionized water, add 4.8mL of 1M hydrochloric acid to the silicon source solution, and stir for 24h. After stirring for 24h, put it in a water bath and heat to evaporate alcohol, the alcohol temperature is 50°C, the alcohol is evaporated for 2.5h, and the amount of alcohol evaporated is 8.5g, to obtain a uniform colloidal solution A.
[0067] Step 2, during the hydrolysis of TEOS, 1.81 g of KOH was weighed and dissolved in 14 g of deionized water, and then 0.835 g of aluminum hydroxide was added to the above solution. After stirring evenly, it was transferred to a stainless steel reactor and moved into a homogeneous reactor. It was dynamically dissolved at 180° C. for 2 h. After being taken out, it was cooled to room temperature in tap water. After opening the reactor, a uniform, stable and transparent solution B was obtained.
[0068] Step 3, then add 4.91g of 25% tetraethylammonium hydroxide solution to solution B under vigorous stirring. Then add colloidal solution A and stir continuously to obtain a silica-alumina mixed gel. The molar composition of the silica-alumina mixed gel is Al2O3:KOH:SiO2:TEAOH:H2O=1:16.4:22:2.68:620.
[0069] Step 4, after further aging for 2 hours, the formed gel was transferred to a 100 mL polytetrafluoroethylene reactor and dynamically crystallized at 170° C. at a speed of 15 r / min for 2 days to obtain a crystallized product containing the template SUZ-4 molecular sieve.
[0070] Step 5, the crystallized product containing the template SUZ-4 molecular sieve is washed with deionized water until it is neutral, dried at 100°C for 8h, and heated to 560°C at a heating rate of 3°C / min for 6h to obtain K-SUZ-4 molecular sieve. Its XRD spectrum is shown in the attached Figure 1 .
[0071] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.
Claims
1. A method for preparing a willow-leaf-shaped K-SUZ-4 molecular sieve, characterized in that: The following steps are involved: Step 1, adding hydrochloric acid and ethyl orthosilicate to deionized water in sequence, stirring to fully hydrolyze, heating to evaporate part of the ethanol, and obtaining a uniform colloidal solution A; Step 2, adding an alkali source and an aluminum source to deionized water in sequence, transferring the mixture to a homogeneous reactor, heating the mixture to fully dissolve the mixture, taking the mixture out and cooling it to room temperature to obtain a uniform and stable solution B; Step 3, adding the directing agent and solution A to solution B in sequence, and stirring vigorously to obtain a uniform silica-alumina mixed gel; Step 4, after continued stirring and aging, the mixture is transferred into a hydrothermal reactor and subjected to dynamic crystallization in a homogeneous reactor, and the crystallization time and temperature are controlled to obtain a crystallized product containing a template SUZ-4 molecular sieve; Step 5, washing, drying and calcining the obtained crystallized product to obtain a willow-leaf-shaped K-type SUZ-4 molecular sieve; The molar ratio of the raw materials in the hydrolysis process of step 1 is H2O: HCl: TEOS=(18-21):(0.015-0.06):(0.8-1.2); In the step 1, the temperature for heating to evaporate ethanol is controlled at 40-60° C., stirring is continued during the process, and the amount of evaporated alcohol accounts for 21 wt.%-32 wt.% of the total solution; In the step 2, the molar ratio of the raw materials in solution B is Al: KOH: H2O=1: (8-9.3): 153; the dissolution temperature is 130-170°C, and the dissolution time is 2-5 h; In step 3, the directing agent is tetraethylammonium hydroxide; The molar ratio of the raw materials in the silica-alumina mixed gel is Al2O3: KOH: SiO2: TEAOH: H2O = 1: (16-19): (18-24): (2-3): (618-671); In the step 4, the aging time is 2 to 5 h, the speed of the homogeneous reactor is 15 to 20 rpm, the crystallization temperature is 160 to 180° C., and the crystallization time is 2 to 5 days.
2. The method for preparing a willow-leaf-shaped K-SUZ-4 molecular sieve according to claim 1, characterized in that: In step 2, the aluminum source is any one of aluminum powder, aluminum hydroxide, and aluminum isopropoxide, and the alkali source is KOH.
3. The method for preparing a willow-leaf-shaped K-SUZ-4 molecular sieve according to claim 1, characterized in that: The drying temperature in step 5 is 100-120° C. and the drying time is 5-8 h; the calcination temperature in step 5 is 550-600° C., the calcination heating rate is 3° C. / min, and the calcination time is 6-10 h.
4. A willow-leaf-shaped K-SUZ-4 molecular sieve prepared by the preparation method according to any one of claims 1 to 3, characterized in that: The willow-leaf-shaped K-SUZ-4 molecular sieve has a c-axis length of 3 μm, a b-axis width of 200-500 nm, and a thickness of less than 100 nm.
Citation Information
Patent Citations
A method for preparing hedgehog-shaped SUZ-4.
CN109626393B
Synthesis method for regulating SUZ-4 molecular sieve morphology
CN109704364A
Heteroatom molecular sieve M-HSUZ-4 catalyst as well as preparation method and application thereof