High alumina silicate glass and its preparation method and application

By adjusting the composition of high aluminosilicate glass and performing chemical strengthening, the mechanical strength and thermal expansion coefficient problems of traditional glass are solved, and a combination of high mechanical strength and low expansion coefficient is achieved, which is suitable for the application of display device cover glass.

CN116282909BActive Publication Date: 2024-10-22QINGYUAN CSG NEW ENERGY SAVING MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310062423.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-10-22
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

Traditional high aluminosilicate glass has poor mechanical strength or high thermal expansion coefficient, making it difficult to bond with soda-lime glass and unable to meet the needs of display device cover glass.

Method used

Preparing a high aluminosilicate glass, the components include 58%~63% SiO2, 16%~20% Al2O3, 12%~16% Na2O, 2%~5% K2O, 2%~5% MgO, 0.5%~1.5% ZrO2 and 1%~3% B2O3, and through chemical strengthening treatment, the mechanical strength and thermal expansion coefficient of the glass are improved.

Benefits of technology

The obtained high aluminosilicate glass has high mechanical strength, low expansion coefficient, surface stress ≥1000MPa, stress layer depth ≥40μm, and broken ball height ≥120cm. It can be used in conjunction with soda-lime glass and is suitable as a cover plate for display devices. Glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a high-aluminum silicate glass. The components of the high-aluminum silicate glass include, by mass percentage, 58% to 63% of SiO2, 16% to 20% of Al2O3, 12% to 16% of Na2O, 2% to 5% of K2O, 2% to 5% of MgO, 0.5% to 1.5% of ZrO2 and 1% to 3% of B2O3. The high-aluminum silicate glass with the mass percentage of the components in the present application has high mechanical strength, a surface stress of ≥1000MPa after chemical strengthening, a stress layer depth of ≥40μm, a falling ball crushing height of ≥120cm, and a thermal expansion coefficient of (86 to 92)×10 ‑7 ℃ ‑1 , which is close to soda-lime glass, can be bonded with soda-lime glass as cover glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of glass production and manufacturing, and in particular to a high-alumina silicate glass and a preparation method and application thereof. Background Art

[0002] The cover glass for display devices is an item that is easy to fall and needs to have sufficiently high mechanical strength. The mechanical strength of soda-lime glass is poor, and the height of the falling ball is low, which is difficult to meet the use requirements. Using high-aluminum silicate glass as the cover glass material can greatly improve the mechanical strength and falling ball performance of the cover glass. For the part of the cover glass that does not bear the main stress, soda-lime glass is used to further reduce the cost. Traditional high-aluminum silicate glass either has poor mechanical strength or a high thermal expansion coefficient, which is difficult to bond with soda-lime glass.

[0003] Therefore, how to obtain a high aluminosilicate glass with both high mechanical strength and low expansion coefficient has always been an urgent problem to be solved. Summary of the invention

[0004] Based on this, it is necessary to provide a high aluminosilicate glass having both high mechanical strength and low expansion coefficient and a preparation method thereof.

[0005] In one aspect of the present application, a high alumina silicate glass is provided, wherein the components of the high alumina silicate glass include, by mass percentage: 58% to 63% SiO 2 , 16%~20% Al 2 O 3 , 12%~16% Na 2 O, 2%~5% K 2 O, 2%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~3% of B 2 O 3 .

[0006] In one embodiment, the composition of the high alumina silicate glass includes, by mass percentage: 58% to 60% SiO 2 , 18%~20% Al 2 O 3 , 12%~15% Na 2 O, 2%~3% K 2 O, 2%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~2% of B 2 O 3 .

[0007] In one embodiment, the composition of the high alumina silicate glass includes, by mass percentage: 58% to 59% SiO2 , 18%~20% Al 2 O 3 , 14%~15% Na 2 O, 2%~2.5% K 2 O, 3%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~1.5% B 2 O 3 .

[0008] In one embodiment, the thermal expansion coefficient of the high alumina silicate glass in the range of 50°C to 300°C is (86-92)×10 -7 ℃ -1 .

[0009] In one embodiment, the softening point of the high alumina silicate glass is 810°C to 825°C.

[0010] In another aspect of the present application, a method for preparing the high-alumina silicate glass is provided, comprising the following steps:

[0011] Weigh the raw materials according to the components, heat them, and prepare a molten liquid;

[0012] The molten liquid is shaped and annealed to prepare the high alumina silicate glass.

[0013] In one embodiment, the heating step includes: heating the raw material to 1660°C~1690°C, keeping the temperature for 4 hours to 8 hours, and then cooling the raw material to 1620°C~1650°C, and keeping the temperature for 1 hour to 2 hours.

[0014] In one embodiment, the annealing conditions include: the annealing temperature is 730° C. to 760° C., and the annealing time is 2 hours to 4 hours.

[0015] In another aspect of the present application, a strengthened glass is provided, which is obtained by chemically strengthening the high-alumina silicate glass.

[0016] In one embodiment, the step of chemical strengthening treatment includes: placing the high-alumina silicate glass in potassium nitrate molten salt, keeping it warm at a temperature of 410° C. to 430° C. for 3 hours to 6 hours.

[0017] In one embodiment, the surface compressive stress of the tempered glass is ≥1000 MPa, and the stress layer depth is ≥40 μm.

[0018] In one embodiment, the falling ball breaking height of the tempered glass is ≥120 cm.

[0019] In another aspect of the present application, a cover glass for a display device is provided, comprising the high-alumina silicate glass or tempered glass.

[0020] The high aluminum silicate glass with the mass percentage of the components in this application has high mechanical strength, the surface stress after chemical strengthening is ≥1000MPa, the stress layer depth is ≥40μm, the falling ball crushing height is ≥120cm, and the thermal expansion coefficient is (86~92)×10 -7 ℃ -1 , which is close to soda-lime glass, can be bonded with soda-lime glass as cover glass. DETAILED DESCRIPTION

[0021] For ease of understanding of the present invention, the application will be described in more detail below. Preferred embodiments of the application are provided hereinafter. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0023] The following is a detailed description of a high-alumina silicate glass provided in the present application and its preparation method and application.

[0024] In one aspect of the present application, a high alumina silicate glass is provided, wherein the components of the high alumina silicate glass include, by mass percentage: 58% to 63% SiO 2 , 16%~20% Al 2 O 3 , 12%~16% Na 2 O, 2%~5% K 2 O, 2%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~3% of B 2 O 3 .

[0025] Silicon dioxide (SiO 2 ) is the main component of the glass skeleton, which can improve the strength of the glass, but it will increase the viscosity of the glass and reduce the corrosion resistance of the glass to the etching solution. 2 When the content of SiO is lower than 58%, the glass forming performance is poor, and the strength and weather resistance are insufficient; when the content of SiO 2When the content of SiO is higher than 63%, the melting and clarification temperature of the glass is high, it is difficult to melt and homogenize, and the tendency of crystallization increases. 2 The mass percentage of SiO is 58%~63%. 2 The mass percentage includes, but is not limited to, 58%, 58.6%, 59%, 59.8%, 60%, 60.3%, 61%, 61.6%, 62% or 63%, preferably 58% to 60%, and further preferably 58% to 59%.

[0026] Alumina (Al 2 O 3 ) can improve the strength of glass and its resistance to etching liquid, and can greatly improve the ion exchange capacity of glass, but it will increase the viscosity of glass and make it more difficult to clarify. 2 O 3 When the mass percentage of Al is less than 16%, the corrosion resistance and ion exchange capacity of the glass are insufficient. 2 O 3 When the mass percentage of Al is higher than 20%, the viscosity of the glass is too high and it is difficult to clarify, the melting quality is reduced, and the various properties of the glass are significantly affected. 2 O 3 The mass percentage of Al is 16%~20%. 2 O 3 The mass percentage includes, but is not limited to, 16%, 16.5%, 17%, 17.4%, 18%, 18.2%, 19%, 19.6% or 20%, preferably 18% to 20%.

[0027] Sodium oxide (Na 2 O) is a necessary component for ion exchange in glass and can also significantly improve the melting properties of glass. 2 When the O content is less than 12%, the glass has poor melting properties. 2 When the content of O is higher than 16%, the weather resistance of the glass deteriorates. 2 The mass percentage of O is 12%~16%. Specifically, Na 2 The mass percentage of O is, but is not limited to, 12%, 12.6%, 13%, 13.4%, 14%, 14.8%, 15%, 15.2%, 15.7% or 16%. Preferably, Na 2 The mass percentage of O is 12% to 15%. More preferably, Na 2 The mass percentage of O is 14%~15%.

[0028] Potassium oxide (K 2O) and Na 2 O also belongs to alkali metal oxides and has similar functions in the glass structure. They are both necessary components for ion exchange in glass. 2 O and Na 2 O compounding can exert the mixed alkali effect, improve the performance of glass, and can be used to improve the melting properties of glass, increase the ion exchange rate in chemical strengthening, and thus increase the surface compressive stress and stress layer depth of glass after strengthening. 2 When the content of O is too high, the weather resistance is reduced and the ion exchange performance of the glass is reduced. Therefore, in the components of the high alumina silicate glass, K 2 The mass percentage of O is 2%~5%. Specifically, K 2 The mass percentage of O is, but is not limited to, 2%, 2.2%, 3%, 3.4%, 4%, 4.5% or 5%. Preferably, K 2 The mass percentage of O is 2-3%, and more preferably, K 2 The mass percentage of O is 2~2.5%. 2 When the mass percentage of O is less than 2%, the glass has poor melting properties and it is difficult to reach the ideal stress layer depth after strengthening. 2 When the mass percentage of O is higher than 5%, the weather resistance of the glass deteriorates and the thermal expansion coefficient is too large.

[0029] Magnesium oxide (MgO) can reduce the viscosity of glass, promote the melting and clarification of glass, reduce the thermal expansion coefficient of glass, and increase the surface compressive stress value of glass after strengthening. If the mass percentage of MgO is less than 2%, the meltability of the glass deteriorates, and it is difficult to achieve the ideal surface compressive stress value after strengthening; if the mass percentage of MgO is higher than 5%, the glass is easy to crystallize, and the material of the glass is too short and difficult to form. Therefore, in the components of the high-alumina silicate glass, the mass percentage of MgO is 2% to 5%. Specifically, the mass percentage of MgO includes but is not limited to 2%, 2.5%, 3%, 3.2%, 3.4%, 3.7%, 4%, 4.3%, 4.8% or 5%. Preferably, the mass percentage of MgO is 3% to 5%.

[0030] Zirconia (ZrO 2 ) can improve the weather resistance of glass and reduce the thermal expansion coefficient of glass, and is an essential component of the above-mentioned high-alumina silicate glass. 2 If the mass percentage of ZrO is less than 0.5%, the weather resistance of the glass is insufficient and the thermal expansion coefficient is too large; 2 If the mass percentage of ZrO is higher than 1.5%, the melting property of the glass will be poor. 2 The mass percentage is 0.5%~1.5%, specifically, ZrO 2The mass percentage includes, but is not limited to, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%.

[0031] Boron oxide (B 2 O 3 ) can reduce the high temperature viscosity and thermal expansion coefficient of glass, but B 2 O 3 It has an inhibitory effect on ion exchange. 2 O 3 When the content is less than 1%, the glass has poor melting properties and a large thermal expansion coefficient. 2 O 3 When the content is higher than 3%, the ion exchange performance of the glass is poor. 2 O 3 The mass percentage of B is 1%~3%. 2 O 3 The mass percentage includes, but is not limited to, 1%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.5%, 2.8% or 3%, preferably 1% to 2%, more preferably 1% to 1.5%.

[0032] In one example, the composition of the high aluminosilicate glass includes, by mass percentage: 58% to 60% SiO 2 , 18%~20% Al 2 O 3 , 12%~15% Na 2 O, 2%~3% K 2 O, 2%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~2% of B 2 O 3 .

[0033] In one example, the composition of the high aluminosilicate glass includes, by mass percentage: 58% to 59% SiO 2 , 18%~20% Al 2 O 3 , 14%~15% Na 2 O, 2%~2.5% K 2 O, 3%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~1.5% B 2 O 3 .

[0034] In one example, the thermal expansion coefficient of the high alumina silicate glass in the range of 50°C to 300°C is (86-92)×10 -7 ℃ -1 The thermal expansion coefficient of mainstream soda-lime glass is about 90×10 -7 ℃ -1 By controlling the thermal expansion coefficient of high alumina silicate glass within the above range, the glass can be better bonded to soda lime glass.

[0035] In one example, the softening point of the high-aluminum silicate glass is 810°C to 825°C. A softening point temperature higher than 810°C can make the glass have better stress relaxation resistance, so that the stress layer depth can be increased by extending the chemical strengthening time, and the attenuation of the surface compressive stress is also smaller; a softening point temperature lower than 825°C can make the glass be bent at a relatively low temperature, reduce mold loss, and increase the service life of the mold.

[0036] In one example, the melting temperature of the high aluminosilicate glass is less than 1700°C.

[0037] In another aspect of the present application, a method for preparing the above-mentioned high-alumina silicate glass is provided, comprising the following steps:

[0038] Weigh the raw materials according to the components, heat them, and prepare a molten liquid;

[0039] The molten liquid is shaped and annealed to prepare the high alumina silicate glass.

[0040] In one example, the heating step includes: heating the raw material to 1660°C~1690°C, keeping the temperature for 4 hours to 8 hours, and then cooling the raw material to 1620°C~1650°C, and keeping the temperature for 1 hour to 2 hours.

[0041] In one example, the molding temperature is 500°C to 550°C.

[0042] In one example, the annealing conditions include: an annealing temperature of 730° C. to 760° C. and a annealing time of 2 hours to 4 hours.

[0043] In another aspect of the present application, a strengthened glass is provided, which is obtained by chemically strengthening the above-mentioned high-alumina silicate glass.

[0044] In one example, the chemical strengthening treatment step includes: placing the high-alumina silicate glass in potassium nitrate molten salt, keeping it warm at a temperature of 410° C. to 430° C. for 3 hours to 6 hours.

[0045] Furthermore, the temperature and holding time of the chemical strengthening are determined according to the following Table 1, where λ=(0.025SiO 2 +0.025Al 2 O 3 )^[0.1Al 2 O 3 +1 / (0.36MgO+0.64B 2 O 3 )]+0.1ZrO 2 +0.2K 2 O

[0046] Each oxide in the formula represents its mass percentage.

[0047] According to the value range of λ, the corresponding chemical strengthening process parameters are selected.

[0048] Table 1 Chemical strengthening process parameters

[0049]

[0050] By selecting the appropriate strengthening process according to the composition, the strengthening performance of glass can be greatly improved.

[0051] In one example, the value of λ is 4.4-6.2.

[0052] In one example, the surface stress of the strengthened glass is ≥1000 MPa.

[0053] In one example, the stress layer depth of the strengthened glass is ≥40 μm.

[0054] In one example, the falling ball breaking height of the tempered glass is ≥120 cm.

[0055] Furthermore, the stress relaxation coefficient ω of the tempered glass is greater than 1.35, and the stress relaxation coefficient ω=(CS6×DOL6) / (CS3×DOL3), wherein CS3 and DOL3 are respectively the surface compressive stress and stress layer depth of the tempered glass obtained by placing the high alumina silicate glass in potassium nitrate molten salt at a temperature of 420°C and keeping warm for 3 hours, and CS6 and DOL6 are respectively the surface compressive stress and stress layer depth of the tempered glass obtained by placing the high alumina silicate glass in potassium nitrate molten salt at a temperature of 420°C and keeping warm for 6 hours.

[0056] In one example, the method for preparing the high alumina silicate glass and the tempered glass comprises the following steps:

[0057] S110: Prepare raw materials: Based on 1400 g of glass liquid, calculate and weigh the raw materials according to the components, grind them, and stir and mix them thoroughly.

[0058] S120: Melting: The mixed raw materials are placed in a crucible for melting. Without limitation, the crucible may be a platinum crucible. The crucible is placed in a lifting furnace, heated to a melting temperature of 1660°C to 1690°C, kept at this temperature for 4 to 8 hours, then cooled to 1620°C to 1650°C, kept at this temperature for 1 to 2 hours, and a molten liquid is prepared.

[0059] S130: Molding: pouring the above molten liquid into a mold for molding and waiting for it to harden. Without limitation, the mold may be a rectangular graphite mold with a size of 200 mm×120 mm. The temperature of the mold during casting is 500°C to 550°C.

[0060] S140: Annealing: The formed sample is placed in an annealing furnace at 730°C to 760°C for 2 to 4 hours to prepare high alumina silicate glass.

[0061] The high aluminosilicate glass was cut into glass sheets with a size of 155 mm×80 mm×1.1 mm, double-sided ground and polished, and CNC processed.

[0062] S150: Chemical strengthening: placing the high alumina silicate glass in potassium nitrate molten salt at a temperature of 410° C. to 430° C. for 3 to 6 hours.

[0063] Performance Test:

[0064] The surface stress value CS and the stress layer depth DOL of the above-mentioned strengthened glass were tested using a FSM-6000LE birefringence stress meter in accordance with the standard GB / T18144-2008. The photoelastic coefficient used in the test was 27.5 nm / (cm·MPa) and the refractive index was 1.51.

[0065] Drop ball breaking height test: Use a steel ball with a mass of 130g to hit the center point of the tempered glass, starting from 30cm and increasing by 5cm each time until the glass breaks, and record the height when it breaks. Repeat the test on 20 pieces of glass from the same batch, and use Weibull distribution fitting to determine the drop ball breaking height B10 value, that is, the glass breaking height under Weibull distribution has a 90% probability of being higher than this value.

[0066] The high temperature viscosity of the glass was tested using an Orton RSV-1600 high temperature viscometer to obtain the temperature viscosity curve data. The VFT formula was used to fit the glass viscosity in the entire temperature range to determine the melting temperature T of the glass. m (Viscosity is 10 2.0 dPa.s temperature) and softening point T s (Viscosity is 10 7.65 dPa.s);

[0067] The high alumina silicate glass was cut into glass sheets with a size of 25 mm×7 mm×1.1 mm, and the thermal expansion coefficient of the glass was tested (50-300° C.) using a NETZSCH DIL-402PC horizontal dilatometer according to GB / T16920-2015 standard.

[0068] It can be understood that the above-mentioned test methods and test equipment are commonly used methods for evaluating glass-related properties in the industry. They are only a means to characterize or evaluate the technical scheme and technical effects of the present invention. Other test methods and test equipment may also be used without affecting the final results.

[0069] In another aspect of the present application, a cover glass for a display device is provided, comprising the above-mentioned high-alumina silicate glass or tempered glass.

[0070] The high aluminum silicate glass with the mass percentage of the components in this application has high mechanical strength, the surface stress after chemical strengthening is ≥1000MPa, the stress layer depth is ≥40μm, the falling ball crushing height is ≥120cm, and the thermal expansion coefficient is (86~92)×10 -7 ℃ -1 , which is close to soda-lime glass, can be bonded with soda-lime glass as cover glass.

[0071] The high-alumina silicate glass and tempered glass and the preparation method thereof provided by the present invention are described in detail below in conjunction with specific embodiments.

[0072] The following are specific embodiments.

[0073] Embodiments 1 to 9

[0074] Examples 1 to 9 all provide high-alumina silicate glass and tempered glass. The specific preparation methods are as follows:

[0075] According to the mass percentage of each component in Table 2, 1400 g of raw materials were weighed, ground and mixed evenly, and then placed in a platinum crucible, which was then placed in a lifting furnace.

[0076] Calculate and weigh the corresponding batch materials based on 1400g of glass liquid, grind and mix them evenly, and place them in a platinum crucible. Place the platinum crucible in a lifting furnace and heat it to 1660℃~1690℃ (T1). Keep it warm for 6 hours and then reduce the temperature to 1620℃~1650℃ (T2). Keep it warm for another 1 hour. Cast it in a rectangular graphite mold with a size of 200mm×120mm and a temperature of 500℃~550℃ (T3). After hardening, transfer it to an annealing furnace at 730℃~760℃ (T4). After keeping it warm for 3 hours, cool it to room temperature with the furnace to obtain high aluminum silicate glass. The specific values ​​of heating temperature T1, T2, molding temperature T3 and annealing temperature T4 are shown in Table 1. In the table:

[0077] λ=(0.025SiO 2 +0.025Al 2 O 3 )^[0.1Al 2 O 3 +1 / (0.36MgO+0.64B 2 O 3 )]+0.1ZrO 2 +0.2K 2 O, where each oxide represents its mass percentage.

[0078] Table 2 Components and preparation process parameters

[0079]

[0080] According to the value range of λ, the corresponding chemical strengthening process parameters are selected. Specifically, as shown in Table 1, when λ>6.0, the 1# strengthening process is adopted, and the high-aluminum silicate glass is placed in potassium nitrate molten salt, and kept warm at a temperature of 430°C for 3.5 hours; when λ is 5.0~6.0, the 2# strengthening process is adopted, and the high-aluminum silicate glass is placed in potassium nitrate molten salt, and kept warm at a temperature of 420°C for 4 hours; when λ<5.0, the 3# strengthening process is adopted, and the high-aluminum silicate glass is placed in potassium nitrate molten salt, and kept warm at a temperature of 410°C for 4.5 hours.

[0081] The thermal properties of the high alumina silicate glasses prepared in Examples 1 to 9 were tested, and the test results are shown in Table 3. Wherein, Tm is the melting temperature of the glass, in °C; Ts is the softening point temperature of the glass, in °C; CTE is the thermal expansion coefficient of the glass at 50 to 300 °C, in ×10 -7 ℃ -1 .

[0082] Table 3 Thermal properties test of high alumina silicate glass

[0083]

[0084] The strengthening performance of the strengthened glass prepared in Examples 1 to 9 was tested, and the test results are shown in Table 4. Wherein, CS is the surface compressive stress value, in MPa; DOL is the maximum stress layer depth, in μm; ω is the stress relaxation coefficient; and the ball drop height B10 value is the value at which the glass breaking height under the Weibull distribution has a 90% probability of being higher than this value, in cm.

[0085] Table 4 Strengthening performance test of tempered glass

[0086]

[0087] From the data in Table 4, it can be seen that the thermal expansion coefficient of the high aluminosilicate glass using the mass percentage of the components in this application is (86~92)×10 -7 ℃ -1 , which is close to soda-lime glass, and can be bonded with soda-lime glass as cover glass; after chemical strengthening, the surface stress is ≥1000MPa, the stress layer depth is ≥40μm, the falling ball crushing height is ≥120cm, and the molten salt temperature during the chemical strengthening process is controlled below 430℃, which is beneficial to prolong the service life of the molten salt, and the strengthening time is shortened by more than 0.5 hours compared with the traditional process, which is beneficial to energy saving and improving processing efficiency.

[0088] Comparative Examples 1 to 9

[0089] The specific preparation methods of the glasses provided in Comparative Examples 1 to 9 are the same as those in Example 1, except that the mass percentages of the components are different. The mass percentages of the components in Comparative Examples 1 to 9 are shown in Table 5 below.

[0090] Table 5 Components

[0091]

[0092] The high alumina silicate glass and tempered glass obtained in Comparative Examples 1 to 8 were tested, and the test results are shown in Table 6.

[0093] Table 6 Glass performance test

[0094]

[0095] From the data in Table 6, we can see that when Al 2 O 3 , MgO or B 2 O 3 When the content of is too high or too low, the CTE of the glasses prepared in Comparative Examples 3, 4, 6 and 8 is lower than 86×10 -7 ℃ -1 , which cannot match soda-lime glass. Moreover, the mechanical strength of comparative examples 1 to 8 is poor, and the B10 values ​​are all lower than 120 cm. This shows that there is a strong synergistic effect between the components of the present application, and as a whole, they jointly bring about the technical effect of the present application.

[0096] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0097] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A tempered glass, It is characterized in that It is obtained by chemically strengthening high-alumina silicate glass in potassium nitrate molten salt; In terms of mass percentage, the high alumina silicate glass is composed of the following components: 58% to 58.6% SiO 2 , 18%~20% Al 2 O 3 , 14%~15% Na 2 O, 2%~2.5% K 2 O, 3%~5% MgO, 0.5%~1.5% ZrO 2 and 1%~1.5% B 2 O 3 ; The temperature and holding time of the chemical strengthening treatment are determined according to the value of λ, where λ = (0.025SiO 2 +0.025Al 2 O 3 )^[0.1Al 2 O 3 +1 / (0.36MgO+0.64B 2 O 3 )]+0.1ZrO 2 +0.2K 2 O, where each oxide represents its mass percentage; Wherein, when λ>6.0, the temperature of the chemical strengthening is 430°C and the strengthening time is 3.5h; When λ is 5.0-6.0, the temperature of the chemical strengthening is 420°C and the strengthening time is 4h; When λ<5.0, the temperature of the chemical strengthening is 410° C., and the strengthening time is 4.5 h.

2. The tempered glass according to claim 1, It is characterized in that The thermal expansion coefficient of the high alumina silicate glass in the range of 50°C to 300°C is (86-92)×10 -7 ℃ -1 .

3. The tempered glass according to claim 1, It is characterized in that The softening point of the high alumina silicate glass is 810°C to 825°C.

4. The tempered glass according to claim 1, It is characterized in that The preparation method of the high alumina silicate glass comprises the following steps: Weigh the raw materials according to the components, heat them, and prepare a molten liquid; The molten liquid is shaped and annealed to prepare the high alumina silicate glass.

5. The tempered glass according to claim 4, It is characterized in that The heating step comprises: heating the raw material to 1660° C. to 1690° C., keeping the temperature for 4 to 8 hours, and then cooling the raw material to 1620° C. to 1650° C., and keeping the temperature for 1 to 2 hours.

6. The tempered glass according to claim 4 or 5, It is characterized in that The annealing conditions include: annealing temperature of 730° C. to 760° C. and annealing time of 2 hours to 4 hours.

7. The tempered glass according to any one of claims 1 to 5, It is characterized in that The surface compressive stress of the tempered glass is ≥1000 MPa, and the stress layer depth is ≥40 μm.

8. The tempered glass according to any one of claims 1 to 5, It is characterized in that The falling ball breaking height of the tempered glass is ≥120 cm.

9. A cover glass for a display device, It is characterized in that The tempered glass comprising the tempered glass according to any one of claims 1 to 8.